Method for preparing silicon carbide ceramic from silicon carbide production waste and silicon carbide ceramic

By using raw materials such as sodium styrene sulfonate, acrylic monomers and allyl polyethers to prepare modifiers under the action of persulfate initiator, the surface modification of silicon carbide powder was solved, and the tightness of silicon carbide ceramics was solved. and the problem of insufficient hardness, efficient waste recycling and environmental protection have been achieved.

CN118930275AActive Publication Date: 2024-11-12JIANGSU CHAOXINXING SEMICON CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411233470.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12
Estimated Expiration
2044-09-04

AI Technical Summary

Technical Problem

In the prior art, the tightness of silicon carbide ceramics is insufficient and the hardness needs to be improved, resulting in low recycling efficiency of silicon carbide production waste.

Method used

Using sodium styrene sulfonate, acrylic monomers and allyl polyether as raw materials, the modifier is prepared under the action of persulfate initiator, and the surface modification of silicon carbide powder is reduced to reduce aggregation and improve dispersion effect. , a modified silicon carbide slurry with low viscosity and good dispersion was finally obtained.

Benefits of technology

The preparation of silicon carbide ceramics with high tightness and high hardness has been achieved, achieving the purpose of saving costs and recycling waste materials, and protecting the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027003570000191
    Figure BDA0005027003570000191
Patent Text Reader

Abstract

The invention provides a method for preparing silicon carbide ceramic from silicon carbide production waste and the silicon carbide ceramic, and the method comprises the following steps: (1) pretreating the silicon carbide production waste to obtain silicon carbide powder; (2) mixing sodium p-styrenesulfonate, sodium hydrogen sulfite, an acrylic monomer, allyl polyether, persulfate and a first solvent to obtain a modifier; and (3) carrying out modification treatment on the silicon carbide powder obtained in the step (1) by using the modifier obtained in the step (2) to obtain modified silicon carbide powder, and preparing the silicon carbide ceramic by using the modified silicon carbide powder. According to the method, sodium p-styrenesulfonate, an acrylic monomer and allyl polyether are used as raw materials, a modifier is obtained under the action of a persulfate initiator, and the modifier is used for surface modification of silicon carbide powder, so that aggregation of the modified silicon carbide powder in the ceramic preparation process is reduced; the ceramic slurry with lower viscosity and good dispersion is obtained, so that the silicon carbide ceramic with higher compactness and higher hardness is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon carbide, and relates to a method for preparing silicon carbide ceramics from silicon carbide production waste, and in particular to a method for preparing silicon carbide ceramics from silicon carbide production waste and silicon carbide ceramics. Background Art

[0002] Among the methods of cutting silicon carbide crystals, multi-wire cutting is one of the more commonly used methods. During the cutting process, a steel wire with diamond particles is used to cut the crystal. The cutting process is bound to cause loss of silicon carbide crystal cutting. The cut silicon carbide powder and diamond will be precipitated in the water together, and waste liquid containing silicon carbide powder and diamond particles will be obtained. On the other hand, during the cutting and grinding of silicon carbide crystals, silicon carbide wafers will also crack, forming silicon carbide wafer waste. These materials are generally treated as waste, resulting in serious waste. On the other hand, during the growth of silicon carbide crystals, some unused silicon carbide powder will pass through, which will also cause a waste of resources.

[0003] In order to enhance the recycling of silicon carbide crystal waste, those skilled in the art use silicon carbide powder to prepare silicon carbide ceramics.

[0004] CN112851356A discloses a method for preparing silicon carbide ceramics by using waste liquid from diamond wire cutting of silicon carbide crystals. In the method, silicon carbide powder and diamond particles in the waste liquid from diamond wire cutting of silicon carbide crystals are cleaned and dried, and then single crystal silicon powder is added to the mixed particles to react with the diamond particles in the mixed particles under heating conditions to produce silicon carbide, thereby obtaining a silicon carbide blank, which is finally fired into silicon carbide ceramics.

[0005] CN102229499A discloses a method for preparing composite antistatic wear-resistant ceramics using silicon carbide / silicon powder discarded after solar silicon wafer wire cutting. In this method, acrylate monomers and silicon carbide powder react under the action of an initiator to form a copolymer resin to prepare the antistatic ceramics.

[0006] CN103086721A discloses a method for preparing silicon carbide ceramics by using silicon carbide solid waste. The method comprises the following steps: pre-treating the silicon wafer cutting waste mortar and taking the solid waste as the raw material; adding polycarbosilane as a sintering aid, loading the mortar into a polyurethane ball mill with anhydrous ethanol as a liquid medium, adding glycerol as a binder, and milling the mortar with high-purity alumina balls; heating to remove the solvent; crushing and sieving to obtain silicon carbide powder coated with polycarbosilane on the surface; pressing the mortar into preforms of various shapes under high pressure; heating the preforms from room temperature to 1000°C after 50 minutes, then heating the preforms to 1200°C at a heating rate of 10°C / min, keeping the temperature for 60 minutes, and cooling the preforms with the furnace to obtain sintered silicon carbide ceramic products.

[0007] The methods disclosed in the prior art for preparing silicon carbide ceramics using silicon carbide production waste have certain defects, such as insufficient compactness of the prepared silicon carbide ceramics and the need to further improve the hardness. Therefore, it is very important to develop a new method for preparing silicon carbide ceramics using silicon carbide production waste and silicon carbide ceramics. Summary of the invention

[0008] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing silicon carbide ceramics from silicon carbide production waste and silicon carbide ceramics; the method provided by the present invention utilizes silicon carbide crystal production waste to prepare silicon carbide ceramics, thereby achieving the purposes of cost saving, waste recycling and environmental protection; the method utilizes sodium styrene sulfonate, acrylic monomers and allyl polyether as raw materials, prepares a modifier under the action of a persulfate initiator, and uses the obtained modifier to perform surface modification on silicon carbide powder, thereby reducing the aggregation of the modified silicon carbide powder in the ceramic preparation process and improving the dispersion effect of the modified silicon carbide powder, and finally obtaining a modified silicon carbide slurry with lower viscosity and better dispersion, thereby obtaining silicon carbide ceramics with higher compactness and higher hardness.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing silicon carbide ceramics from silicon carbide production waste, the method comprising:

[0011] (1) Pre-treating silicon carbide production waste to obtain silicon carbide powder;

[0012] (2) mixing a sulfonate containing a polymerizable double bond, an acrylic acid monomer, an allyl polyether, a persulfate, a sulfite, and a first solvent to obtain a modifier;

[0013] (3) modifying the silicon carbide powder obtained in step (1) with the modifier obtained in step (2) to obtain modified silicon carbide powder, and preparing silicon carbide ceramics with the modified silicon carbide powder;

[0014] There is no order of precedence between step (1) and step (2).

[0015] In step (2) of the present invention, under the action of the initiator persulfate and the regulator sulfite, the double bonds in the sodium styrene sulfonate, acrylic acid monomer and allyl polyether generate free radicals in the first solvent, and complete the free radical polymerization reaction.

[0016] The sulfonate containing polymerizable double bonds in the present invention can improve the dispersibility of silicon carbide powder, so that the modified silicon carbide powder exhibits better dispersibility in the process of preparing silicon carbide ceramics; in addition, the double bonds in the sulfonate containing polymerizable double bonds can also undergo polymerization reaction with sodium vinyl sulfonate and acrylic acid monomer.

[0017] The acrylic monomer described in the present invention will polymerize during the process of preparing the modifier, and has certain defoaming and degassing properties after polymerization. When the modified silicon carbide powder is used to prepare silicon carbide ceramics, the bubbles in the slurry can be further eliminated to form a uniform and compact embryo, thereby obtaining a silicon carbide ceramic with high hardness.

[0018] The end of the allyl polyether in the present invention contains a hydroxyl group, which can be connected to the silanol group on the surface of the silicon carbide powder through hydrogen bonding during the modification of the silicon carbide powder to modify the silicon carbide powder. At the same time, the allyl polyether also has a certain length of polyoxyethylene ether chain segments, which can effectively separate the silicon carbide powder, thereby further improving the dispersibility of the modified silicon carbide powder in the process of preparing silicon carbide ceramics.

[0019] The persulfate in the present invention is an initiator in the reaction process, and the persulfate provides free radicals to initiate the reaction.

[0020] The sulfite in the present invention has reducing properties. Sodium bisulfite can not only adjust the free radical concentration in the obtained modifier, but also play an antioxidant role and promote the degree of free radical polymer reaction, so that the modified silicon carbide powder shows a better dispersion effect in the process of preparing silicon carbide ceramics.

[0021] The method provided by the present invention utilizes the production waste of silicon carbide crystals to prepare silicon carbide ceramics, thereby achieving the purposes of cost saving, waste recycling and environmental protection; the method utilizes sulfonates containing polymerizable double bonds, acrylic monomers and allyl polyethers as raw materials, prepares a modifier under the action of a persulfate initiator and a sulfite regulator, and uses the obtained modifier to perform surface modification on silicon carbide powder, thereby reducing the aggregation of the modified silicon carbide powder in the ceramic preparation process, improving the dispersion effect of the modified silicon carbide powder, and finally obtaining a modified silicon carbide slurry with lower viscosity and better dispersion, thereby obtaining silicon carbide ceramics with higher compactness and higher hardness.

[0022] Preferably, the silicon carbide production waste in step (1) includes waste liquid generated during the silicon carbide crystal cutting process, split pieces generated during the silicon carbide crystal processing process, and silicon carbide powder remaining during the silicon carbide crystal growth process.

[0023] Preferably, the pretreatment in step (1) includes pretreating the waste liquid generated during the silicon carbide crystal cutting process, the fragments generated during the silicon carbide crystal processing process, and the silicon carbide powder remaining during the silicon carbide crystal growth process, respectively, to obtain three pretreated silicon carbide powders, and then mixing and grinding the three pretreated silicon carbide powders to obtain silicon carbide powder.

[0024] Preferably, the pretreatment includes sequentially filtering and acid-washing and drying the waste liquid generated during the silicon carbide crystal cutting process to obtain mixed particles of silicon carbide and diamond; then adding single crystal silicon powder to the obtained mixed particles, and then heating the mixed particles to allow the single crystal silicon powder to react with the diamond in the mixed particles to generate silicon carbide.

[0025] Preferably, the molar amount of the single crystal silicon powder added is the same as the molar amount of diamond in the mixed particles; the diamond content in the mixed particles is determined by infrared spectroscopy and / or Raman spectroscopy, and the molar amount of diamond in the mixed particles is then calculated by the diamond content.

[0026] Preferably, the pretreatment includes crushing the fragments generated during the processing of the silicon carbide crystal.

[0027] Preferably, the pretreatment comprises sequentially calcining, acid washing and alkali washing the silicon carbide powder remaining in the silicon carbide crystal growth process.

[0028] The function of the roasting in the present invention is to remove the carbon element, and the roasting temperature is 2000-2200° C. and the time is 2-6 hours.

[0029] The calcination temperature in the present invention is 2000-2200°C, for example, it can be 2000°C, 2020°C, 2040°C, 2060°C, 2080°C, 2100°C, 2120°C, 2140°C, 2160°C, 2180°C or 2200°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] The calcination time in the present invention is 2 to 6 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] The role of the pickling in the present invention is to remove trace elements. The acid used in the pickling includes any one of nitric acid, hydrochloric acid, hydrofluoric acid or sulfuric acid, or a combination of at least two. Typical but non-limiting combinations include a combination of nitric acid and hydrochloric acid, a combination of hydrochloric acid and hydrofluoric acid, a combination of hydrofluoric acid and sulfuric acid, or a combination of nitric acid, hydrochloric acid and hydrofluoric acid.

[0032] The role of the alkali washing in the present invention is to remove silicon element. The reagent used in the alkali washing includes any one of sodium hydroxide, potassium hydroxide, sodium carbonate or potassium carbonate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of sodium hydroxide and potassium hydroxide, a combination of potassium hydroxide and sodium carbonate, a combination of sodium carbonate and potassium carbonate, or a combination of sodium hydroxide, potassium hydroxide and sodium carbonate.

[0033] Preferably, the average particle size of the silicon carbide powder obtained in step (1) is less than 200 μm, for example, it can be 199 μm, 190 μm, 180 μm, 170 μm, 160 μm, 150 μm, 140 μm, 130 μm, 120 μm, 110 μm, 100 μm, 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm, 20 μm or 10 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably less than 50 μm.

[0034] Preferably, the mixing in step (2) comprises: first mixing a sulfonate containing a polymerizable double bond, a sulfite and a first solvent to obtain a first mixture; second mixing an acrylic acid monomer and an allyl polyether to obtain a second mixture; third mixing a persulfate and the first solvent to obtain a third mixture; and fourth mixing the first mixture, the second mixture and the third mixture, adjusting the pH and then drying to obtain a modifier.

[0035] Preferably, the fourth mixing comprises: adding the second mixed material and the third mixed material into the first mixed material at a constant flow rate at 60-100° C., keeping the mixture warm after the addition is completed, and then cooling to 15-30° C.

[0036] The fourth mixing step in the present invention is to add the second mixture and the third mixture to the first mixture at a constant flow rate at 60-100°C, for example, it can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the constant flow rate is 0.1-1 ml / min, for example, it can be 0.1 ml / min, 0.2 ml / min, 0.3 ml / min, 0.4 ml / min, 0.5 ml / min, 0.6 ml / min, 0.7 ml / min, 0.8 ml / min, 0.9 ml / min or 1 ml / min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the insulation time is 1 to 3 hours, for example, it can be 1h, 1.2h, 1.41h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the pH is adjusted to 7-8, for example, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9 or 8, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the reagent used to adjust the pH is a base.

[0041] Preferably, the drying method comprises spray drying.

[0042] Preferably, in parts by weight, in the mixing process of step (2), the weight portion of sodium styrene sulfonate is 90 to 110 parts, the weight portion of sulfite is 0.21 to 2.3 parts, the weight portion of acrylic acid monomer is 100 to 300 parts, the weight portion of allyl polyether is 20 to 50 parts, and the weight portion of persulfate is 0.42 to 4.6 parts.

[0043] In the present invention, the weight parts of sodium styrene sulfonate in the mixing process of step (2) is 90 to 110 parts by weight, for example, it can be 90 parts, 92 parts, 94 parts, 96 parts, 98 parts, 100 parts, 102 parts, 104 parts, 106 parts, 108 parts or 110 parts, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In the present invention, the weight parts of sulfite in the mixing process of step (2) is 0.21 to 2.3 parts by weight, for example, it can be 0.21 parts, 0.5 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2 parts, 2.1 parts or 2.3 parts, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] In the present invention, the weight parts of the acrylic acid monomer in the mixing process of step (2) is 100 to 300 parts by weight, for example, it can be 100 parts, 120 parts, 140 parts, 160 parts, 180 parts, 200 parts, 220 parts, 240 parts, 260 parts, 280 parts or 300 parts, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0046] In the present invention, the weight parts of allyl polyether in the mixing process of step (2) is 20 to 50 parts by weight, for example, it can be 20 parts, 22 parts, 25 parts, 27 parts, 30 parts, 32 parts, 35 parts, 37 parts, 40 parts, 42 parts, 45 parts, 48 ​​parts or 50 parts, but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] In the present invention, the weight parts of persulfate in the mixing process of step (2) is 0.42 to 4.6 parts by weight, for example, it can be 0.42 parts, 0.6 parts, 0.8 parts, 1 parts, 1.2 parts, 1.5 parts, 1.7 parts, 2 parts, 2.3 parts, 2.5 parts, 2.7 parts, 3 parts, 3.2 parts, 3.5 parts, 3.8 parts, 4 parts, 4.2 parts, 4.4 parts or 4.6 parts, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0048] In the present invention, the weight of the first solvent in the mixing process of step (2) is not limited, and the amount of the first solvent used can meet the requirements for the polymerization reaction.

[0049] Preferably, the sulfonate containing polymerizable double bonds comprises any one of sodium styrene sulfonate, sodium acrylic acid sulfonate, sodium methacrylic acid sulfonate, sodium 2-acrylamide-2-methylpropane sulfonate or sodium maleic anhydride sulfonate or a combination of at least two thereof. Typical but non-limiting combinations include a combination of sodium styrene sulfonate and sodium acrylic acid sulfonate, a combination of sodium methacrylic acid sulfonate and sodium 2-acrylamide-2-methylpropane sulfonate, a combination of sodium styrene sulfonate and sodium maleic anhydride sulfonate, or a combination of sodium styrene sulfonate, sodium acrylic acid sulfonate and sodium methacrylic acid sulfonate, preferably sodium styrene sulfonate.

[0050] Preferably, the acrylic monomer comprises any one of acrylic acid, methacrylic acid, methyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate or isooctyl acrylate, or a combination of at least two thereof, preferably a combination of hydroxyethyl acrylate and isooctyl acrylate. Typical but non-limiting combinations include a combination of acrylic acid and methacrylic acid, a combination of methyl methacrylate and hydroxyethyl acrylate, a combination of hydroxypropyl acrylate and hydroxybutyl acrylate, a combination of hydroxybutyl acrylate and isooctyl acrylate, or a combination of methacrylic acid, methyl methacrylate and hydroxyethyl acrylate.

[0051] Preferably, the persulfate comprises any one of potassium persulfate, ammonium persulfate or sodium persulfate, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of potassium sulfate and ammonium persulfate, a combination of ammonium persulfate and sodium persulfate, or a combination of potassium persulfate, ammonium persulfate and sodium persulfate.

[0052] Preferably, the sulfite comprises any one or a combination of at least two of sodium sulfite, sodium bisulfite, potassium sulfite or calcium sulfite. Typical but non-limiting combinations include a combination of sodium sulfite and sodium bisulfite, a combination of potassium sulfite and calcium sulfite, or a combination of sodium sulfite, sodium bisulfite and potassium sulfite, preferably sodium bisulfite.

[0053] Preferably, the molecular formula of the allyl polyether is CH2CHCH2(C2H4O) m H; wherein m is 2 to 10, for example, 2, 3, 4, 5, 6, 7, 8, 9 or 10, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 6 to 10.

[0054] Preferably, the first solvent comprises any one of water, ethanol or isopropanol or a combination of at least two of them. Typical but non-limiting combinations include a combination of water and ethanol, a combination of ethanol and isopropanol, or a combination of water, ethanol and isopropanol.

[0055] Preferably, the modification treatment in step (3) comprises:

[0056] The silicon carbide powder obtained in step (1) is mixed with the second solvent and the pH is adjusted to obtain a primary mixture. The primary mixture is then mixed with the modifier obtained in step (2) and heated to the end temperature and stirred while being kept warm. After solid-liquid separation, modified silicon carbide powder is obtained.

[0057] Preferably, the mass ratio of the silicon carbide powder to the second solvent is (30-50):100, for example, it can be 30:100, 32:100, 35:100, 37:100, 40:100, 42:100, 45:100, 47:100 or 50:100, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0058] Preferably, the second solvent comprises any one of water, ethanol or isopropanol or a combination of at least two of them. Typical but non-limiting combinations include a combination of water and ethanol, a combination of ethanol and isopropanol, or a combination of water, ethanol and isopropanol.

[0059] Preferably, the mass ratio of the primary mixture to the modifier is 100:(0.5-1), for example, it can be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9 or 100:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0060] Preferably, the pH is adjusted to 9-10, for example, 9, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9 or 10, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0061] Preferably, the endpoint temperature is 60-80°C, for example, it can be 60°C, 62°C, 65°C, 68°C, 70°C, 72°C, 75°C, 78°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0062] Preferably, the stirring time is 0.5 to 1 h, for example, 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h or 1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0063] Preferably, the solid-liquid separation method includes filtration.

[0064] Preferably, in step (3), preparing silicon carbide ceramics using the obtained modified silicon carbide powder comprises:

[0065] The modified silicon carbide powder, surfactant and defoamer are mixed to obtain ceramic slurry, and the obtained ceramic slurry is sintered to obtain silicon carbide ceramics.

[0066] Preferably, the mass ratio of the modified silicon carbide powder, the surfactant and the defoaming agent is 100:(0.5-1):(0.5-1).

[0067] The mass ratio of the modified silicon carbide powder to the surfactant in the present invention is 100:(0.5-1), for example, it can be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9 or 100:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] The mass ratio of the modified silicon carbide powder to the defoaming agent in the present invention is 100:(0.5-1), for example, it can be 100:0.5, 100:0.6, 100:0.7, 100:0.8, 100:0.9 or 100:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0069] Preferably, the surfactant comprises any one of sodium dodecyl sulfate, sodium dodecyl sulfonate or sodium dodecylbenzene sulfonate or a combination of at least two thereof, and typical but non-limiting combinations include a combination of sodium dodecyl sulfate and sodium dodecyl sulfonate, a combination of sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate, or a combination of sodium dodecyl sulfate, sodium dodecyl sulfonate and sodium dodecylbenzene sulfonate.

[0070] Preferably, the defoamer comprises any one of a polyether defoamer, a mineral oil defoamer or a silicone defoamer, or a combination of at least two of them. Typical but non-limiting combinations include a combination of a polyether defoamer and a mineral oil defoamer, a combination of a mineral oil defoamer and a silicone defoamer, or a combination of a polyether defoamer, a mineral oil defoamer and a silicone defoamer.

[0071] Preferably, the sintering molding comprises: injecting the obtained ceramic slurry into a mold, then performing vibration and vacuum suction in sequence to remove foam, and then performing sintering treatment.

[0072] Preferably, the sintering treatment is carried out at a temperature of 2000-2400° C. and for a time of 2-6 hours.

[0073] The temperature of the sintering treatment in the present invention is 2000-2400°C, for example, it can be 2000°C, 2050°C, 2100°C, 2150°C, 2200°C, 2250°C, 2300°C, 2350°C or 2400°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0074] The sintering time in the present invention is 2 to 6 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, 5.5 hours or 6 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0075] As a preferred technical solution of the method of the present invention, the method comprises:

[0076] (1) The waste liquid generated during the silicon carbide crystal cutting process is sequentially graded and filtered and pickled and dried to obtain mixed particles of silicon carbide and diamond; single crystal silicon powder is added to the obtained mixed particles, and then heated to allow the single crystal silicon powder to react with the diamond in the mixed particles to generate silicon carbide, thereby obtaining a first pretreated silicon carbide powder;

[0077] Crushing the fragments generated during the processing of the silicon carbide crystal to obtain a second pretreated silicon carbide powder;

[0078] The silicon carbide powder remaining in the process of silicon carbide crystal growth is sequentially roasted, acid-washed and alkaline-washed to obtain a third pretreated silicon carbide powder;

[0079] The first pretreated silicon carbide powder, the second pretreated silicon carbide powder and the third pretreated silicon carbide powder are mixed and then ground to obtain silicon carbide powder with an average particle size of less than 50 μm;

[0080] (2) In parts by weight, a first mixture of 90 to 110 parts by weight of a sulfonate containing a polymerizable double bond, 0.21 to 2.3 parts by weight of a sulfite and 500 to 900 parts by weight of a first solvent is prepared to obtain a first mixture; a second mixture of 100 to 300 parts by weight of an acrylic acid monomer and 20 to 50 parts by weight of an allyl polyether is prepared to obtain a second mixture; a third mixture of 0.42 to 4.6 parts by weight of a persulfate and 50 to 100 parts by weight of the first solvent is prepared to obtain a third mixture; and the second mixture and the third mixture are added to the first mixture at a constant flow rate of 0.1 to 1 ml / min at 60 to 100° C., and after the addition is completed, the mixture is kept warm for 1 to 3 hours, and then cooled to 15 to 30° C., the pH is adjusted to 7 to 8, and then spray-dried to obtain a modifier;

[0081] (3) mixing the silicon carbide powder obtained in step (1) and the second solvent in a mass ratio of (30-50):100, adjusting the pH to 9-10 to obtain a primary mixture, and then mixing the primary mixture with the modifier obtained in step (2) in a mass ratio of 100:(0.5-1), heating to 60-80° C., stirring for 0.5-1 h, and filtering to obtain modified silicon carbide powder;

[0082] The modified silicon carbide powder, a surfactant and a defoamer in a mass ratio of 100:(0.5-1):(0.5-1) are mixed to obtain a ceramic slurry, the obtained ceramic slurry is injected into a mold, and then vibration and vacuum suction are performed in sequence to remove foam, and then sintering treatment is performed at 2000-2400° C. for 2-6 hours to obtain silicon carbide ceramics;

[0083] There is no order of precedence between step (1) and step (2).

[0084] In a second aspect, the present invention provides a silicon carbide ceramic, which is obtained by the method described in the first aspect.

[0085] Compared with the prior art, the present invention has the following beneficial effects:

[0086] The method provided by the present invention utilizes production waste of silicon carbide crystals to prepare silicon carbide ceramics, thereby achieving the purposes of cost saving, waste recycling and environmental protection; the method utilizes sodium styrene sulfonate, acrylic monomers and allyl polyether as raw materials, prepares a modifier under the action of a persulfate initiator, and uses the obtained modifier to perform surface modification on silicon carbide powder, thereby reducing the aggregation of the modified silicon carbide powder in the ceramic preparation process and improving the dispersion effect of the modified silicon carbide powder, and finally obtaining a modified silicon carbide slurry with lower viscosity and better dispersion, thereby obtaining silicon carbide ceramics with higher compactness and higher hardness. DETAILED DESCRIPTION

[0087] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0088] Example 1

[0089] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, the method comprising:

[0090] (1) The waste liquid generated during the silicon carbide crystal cutting process is sequentially graded and filtered and pickled and dried to obtain mixed particles of silicon carbide and diamond; single crystal silicon powder is added to the obtained mixed particles, and then heated to allow the single crystal silicon powder to react with the diamond in the mixed particles to generate silicon carbide, thereby obtaining a first pretreated silicon carbide powder;

[0091] Crushing the fragments generated during the processing of the silicon carbide crystal to obtain a second pretreated silicon carbide powder;

[0092] The silicon carbide powder remaining in the process of silicon carbide crystal growth is sequentially roasted, acid-washed and alkaline-washed to obtain a third pretreated silicon carbide powder;

[0093] The first pretreated silicon carbide powder, the second pretreated silicon carbide powder and the third pretreated silicon carbide powder are mixed and ground to obtain silicon carbide powder with an average particle size of 35 μm;

[0094] (2) In parts by weight, 100 parts of sodium styrene sulfonate, 1 part of sodium bisulfite and 700 parts of water are mixed to obtain a first mixture; 200 parts of acrylic acid monomer and 35 parts of allyl polyether are mixed to obtain a second mixture; 2 parts of sodium persulfate and 75 parts of water are mixed to obtain a third mixture; and the second mixture and the third mixture are added to the first mixture at a constant flow rate of 0.5 ml / min at 80° C., and after the addition is completed, the mixture is kept warm for 2 hours, cooled to 24° C., adjusted to pH 7.5, and then spray-dried to obtain a modifier;

[0095] (3) mixing the silicon carbide powder obtained in step (1) with water in a mass ratio of 40:100, adjusting the pH to 9.5 to obtain a primary mixture, and then mixing the primary mixture with the modifier obtained in step (2) in a mass ratio of 100:0.7, heating to 75° C., stirring for 0.75 h, and filtering to obtain modified silicon carbide powder;

[0096] The modified silicon carbide powder, sodium dodecyl sulfate and polyether defoamer in a mass ratio of 100:0.75:0.75 were mixed to obtain a ceramic slurry, the obtained ceramic slurry was injected into a mold, and then vibration and vacuum suction were performed in sequence to remove foam, and then sintering treatment was performed at 2200° C. for 4 hours to obtain silicon carbide ceramics;

[0097] There is no order of precedence between step (1) and step (2).

[0098] Example 2

[0099] (1) The waste liquid generated during the silicon carbide crystal cutting process is sequentially graded and filtered and pickled and dried to obtain mixed particles of silicon carbide and diamond; single crystal silicon powder is added to the obtained mixed particles, and then heated to allow the single crystal silicon powder to react with the diamond in the mixed particles to generate silicon carbide, thereby obtaining a first pretreated silicon carbide powder;

[0100] Crushing the fragments generated during the processing of the silicon carbide crystal to obtain a second pretreated silicon carbide powder;

[0101] The silicon carbide powder remaining in the process of silicon carbide crystal growth is sequentially roasted, acid-washed and alkaline-washed to obtain a third pretreated silicon carbide powder;

[0102] The first pretreated silicon carbide powder, the second pretreated silicon carbide powder and the third pretreated silicon carbide powder are mixed and ground to obtain silicon carbide powder with an average particle size of 20 μm;

[0103] (2) In parts by weight, 90 parts by weight of sodium acrylic acid sulfonate, 0.21 parts by weight of sodium sulfite and 500 parts by weight of water are mixed to obtain a first mixture; 100 parts by weight of acrylic acid monomer and 20 parts by weight of allyl polyether are mixed to obtain a second mixture; 0.42 parts by weight of potassium persulfate and 50 parts by weight of ethanol are mixed to obtain a third mixture; and the second mixture and the third mixture are added to the first mixture at a constant flow rate of 1 ml / min at 60° C., and after the addition is completed, the mixture is kept warm for 3 hours, cooled to 30° C., adjusted to pH 7, and then spray-dried to obtain a modifier;

[0104] (3) mixing the silicon carbide powder obtained in step (1) with water in a mass ratio of 30:100, adjusting the pH to 9 to obtain a primary mixture, and then mixing the primary mixture with the modifier obtained in step (2) in a mass ratio of 100:1, heating to 80° C., stirring for 0.5 h, and filtering to obtain modified silicon carbide powder;

[0105] The modified silicon carbide powder, sodium dodecyl sulfate and mineral oil defoamer in a mass ratio of 100:1:0.5 are mixed to obtain a ceramic slurry, the obtained ceramic slurry is injected into a mold, and then vibration and vacuum suction are performed in sequence to remove foam, and then sintering treatment is performed at 2400° C. for 2 hours to obtain silicon carbide ceramics;

[0106] There is no order of precedence between step (1) and step (2).

[0107] Example 3

[0108] (1) The waste liquid generated during the silicon carbide crystal cutting process is sequentially graded and filtered and pickled and dried to obtain mixed particles of silicon carbide and diamond; single crystal silicon powder is added to the obtained mixed particles, and then heated to allow the single crystal silicon powder to react with the diamond in the mixed particles to generate silicon carbide, thereby obtaining a first pretreated silicon carbide powder;

[0109] Crushing the fragments generated during the processing of the silicon carbide crystal to obtain a second pretreated silicon carbide powder;

[0110] The silicon carbide powder remaining in the process of silicon carbide crystal growth is sequentially roasted, acid-washed and alkaline-washed to obtain a third pretreated silicon carbide powder;

[0111] The first pretreated silicon carbide powder, the second pretreated silicon carbide powder and the third pretreated silicon carbide powder are mixed and ground to obtain silicon carbide powder with an average particle size of 48 μm;

[0112] (2) In parts by weight, 110 parts by weight of sodium methacrylic acid sulfonate, 2.3 parts by weight of potassium sulfite and 900 parts by weight of ethanol are mixed to obtain a first mixture; 300 parts by weight of acrylic acid monomer and 50 parts by weight of allyl polyether are mixed to obtain a second mixture; 4.6 parts by weight of potassium persulfate and 100 parts by weight of water are mixed to obtain a third mixture; and the second mixture and the third mixture are added to the first mixture at a constant flow rate of 0.1 ml / min at 100° C., and after the addition is completed, the mixture is kept warm for 1 hour, cooled to 15° C., adjusted to pH 8, and then spray-dried to obtain a modifier;

[0113] (3) mixing the silicon carbide powder obtained in step (1) with ethanol in a mass ratio of 50:100, adjusting the pH to 10 to obtain a primary mixture, and then mixing the primary mixture with the modifier obtained in step (2) in a mass ratio of 100:0.5, heating to 60° C., stirring for 1 hour, and filtering to obtain modified silicon carbide powder;

[0114] The modified silicon carbide powder, sodium dodecylbenzene sulfonate and an organosilicon defoamer in a mass ratio of 100:0.5:1 are mixed to obtain a ceramic slurry, the obtained ceramic slurry is injected into a mold, and then vibration and vacuum suction are performed in sequence to remove foam, and then sintering treatment is performed at 2000° C. for 6 hours to obtain silicon carbide ceramics;

[0115] There is no order of precedence between step (1) and step (2).

[0116] Example 4

[0117] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as that of Example 1 except that the average particle size of the silicon carbide powder obtained after grinding in step (1) is 250 μm.

[0118] Example 5

[0119] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as that of Embodiment 1 except that in step (2), the second mixed material and the third mixed material are added to the first mixed material at 40°C.

[0120] Example 6

[0121] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as that of Embodiment 1 except that in step (2), the second mixed material and the third mixed material are added to the first mixed material at 120°C.

[0122] Example 7

[0123] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as Example 1 except that the mass ratio of the initial mixture to the modifier obtained in step (2) during remixing in step (3) is 100:0.2.

[0124] Example 8

[0125] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as that of Example 1 except that the mass ratio of the initial mixture to the modifier obtained in step (2) during remixing in step (3) is 100:1.5.

[0126] Example 9

[0127] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as that of Embodiment 1 except that in step (3), the mixing is repeated, the mixture is heated to 40° C., and then stirred.

[0128] Example 10

[0129] This embodiment provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as that of Embodiment 1 except that in step (3), the mixture is heated to 100° C. and then stirred.

[0130] Comparative Example 1

[0131] This comparative example provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as Example 1 except that the sodium styrene sulfonate in step (2) is omitted.

[0132] Comparative Example 2

[0133] This comparative example provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as Example 1 except that the sodium bisulfite in step (2) is omitted.

[0134] Comparative Example 3

[0135] This comparative example provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as Example 1 except that the acrylic acid monomer in step (2) is omitted.

[0136] Comparative Example 4

[0137] This comparative example provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as Example 1 except that the allyl polyether in step (2) is omitted.

[0138] Comparative Example 5

[0139] This comparative example provides a method for preparing silicon carbide ceramics from silicon carbide production waste, which is the same as Example 1 except that the sodium persulfate in step (2) is omitted.

[0140] Comparative Example 6

[0141] The present comparative example provides a method for preparing silicon carbide ceramics from silicon carbide production waste, except that step (2) is omitted, and in step (3), the silicon carbide powder obtained in step (1) and the second solvent are mixed in a mass ratio of 40:100, the pH is adjusted to 9.5 to obtain a primary mixture, the primary mixture is then mixed with the modifier obtained in step (2) in a mass ratio of 100:0.7, and then heated to 75°C and stirred for 0.75h, and the modified silicon carbide powder is obtained after filtering, that is, the silicon carbide ceramics are directly prepared using the silicon carbide powder obtained in step (1), and the rest is the same as the embodiment.

[0142] Silicon carbide ceramics were prepared by the method for preparing silicon carbide ceramics from silicon carbide production waste provided in the above embodiments and comparative examples, the dispersibility of the ceramic slurry obtained in step (3) was evaluated, and the compactness and hardness of the silicon carbide ceramics finally obtained by sintering were evaluated;

[0143] The evaluation method of the dispersibility of the ceramic slurry includes a viscosity test. The better the dispersibility of the ceramic slurry is, the better the fluidity is, and the corresponding viscosity is lower. The test method of the viscosity of the ceramic slurry is: the viscosity of the ceramic slurry is tested using a rheometer, and the test results are shown in Table 1;

[0144] The evaluation method of the dispersibility of the ceramic slurry also includes a viscosity test after standing. The smaller the viscosity change of the ceramic slurry after standing, the better the dispersibility. The test method of the viscosity of the ceramic slurry after standing for 24 hours is: the viscosity of the ceramic slurry is tested again after standing for 24 hours. The test results are shown in Table 1.

[0145] The evaluation method of the tightness of silicon carbide ceramics includes a bulk density test. The higher the bulk density, the higher the tightness. The test method of the bulk density of silicon carbide ceramics is: national standard GB / T 25995-2010 "Test method for density and apparent porosity of fine ceramics", and the test results are shown in Table 1;

[0146] The Vickers hardness test method of the silicon carbide ceramic is: using a Vickers hardness tester to test the hardness of the ceramic sample. The test results are shown in Table 1.

[0147] Table 1

[0148]

[0149] From Table 1, we can get:

[0150] (1) The silicon carbide ceramics prepared by the methods provided in Examples 1 to 3 of the present invention have high density and hardness;

[0151] (2) By comparing Example 1 with Example 4, it can be seen that the average particle size of the silicon carbide powder obtained after grinding in step (1) of the present invention will affect the performance of the obtained ceramic slurry and silicon carbide ceramics; when the average particle size of the silicon carbide powder is less than 200 μm, the obtained ceramic slurry has a lower viscosity and better dispersion, and the obtained silicon carbide ceramics have excellent performance. This is because when the particle size of the silicon carbide powder is too large, it is easy to agglomerate in the dispersion system, affecting the dispersibility. At the same time, the larger particles have a smaller specific surface area and less interaction with the modifier, resulting in uneven dispersion, which affects the final compactness and hardness of the silicon carbide ceramics.

[0152] (3) By comparing Example 1 with Examples 5 and 6, it can be seen that the temperature at which the second mixed material and the third mixed material are added to the first mixed material in step (2) of the present invention affects the performance of the obtained ceramic slurry and silicon carbide ceramics; when the temperature is 60-100°C, the obtained ceramic slurry has a lower viscosity and better dispersion, and the obtained silicon carbide ceramics have excellent performance. This is because during the polymerization reaction of the modifier, if the reaction temperature is too low, the generation rate of free radicals will be reduced, and the polymerization effect of the final modifier will be reduced; if the reaction temperature is too high, the initiator will decompose too quickly, resulting in a decrease in the utilization rate of the initiator, and the high temperature may introduce unnecessary side reactions, affecting the final performance of the modifier;

[0153] (4) By comparing Example 1 with Examples 7 and 8, it can be seen that the mass ratio of the initial mixture to the modifier obtained in step (2) during remixing in step (3) of the present invention will affect the performance of the obtained ceramic slurry and silicon carbide ceramics; when the mass ratio of the initial mixture to the modifier is 100:(0.5-1), the obtained ceramic slurry has a lower viscosity and better dispersion, and the obtained silicon carbide ceramics have excellent performance. This is because when the amount of modifier is too small, the surface of the mixture cannot be fully modified, and the dispersion performance will naturally decrease, which will eventually affect the dispersibility of the slurry and the final compactness and hardness of the ceramic; when the amount of modifier is too much, the hydroxyl groups in the modifier structure cannot be consumed by hydrogen bonding with the hydroxyl groups on the surface of silicon carbide, and the modifier itself may form hydrogen bonding to form self-aggregation, thereby affecting the dispersion performance of the silicon carbide ceramic slurry, and ultimately affecting the compactness and hardness of the silicon carbide ceramic;

[0154] (5) By comparing Example 1 with Examples 9 and 10, it can be seen that the terminal temperature of the heating after mixing in step (3) of the present invention will affect the performance of the obtained ceramic slurry and silicon carbide ceramics; when the terminal temperature of heating is 60-80°C, the obtained ceramic slurry has a lower viscosity and better dispersion, and the obtained silicon carbide ceramics have excellent performance. This is because when the temperature is 60-80°C during the modification process, it is more conducive to the dispersion of silicon carbide powder, so that it can better contact with the modified material, thereby improving the modification efficiency. On the contrary, too low a temperature will affect the modification efficiency. On the other hand, if the reaction temperature is too high, the chemical bonding strength of the modification process will be weakened, and ultimately the modification effect of the modifier will be weakened, thereby affecting the dispersion performance of the silicon carbide ceramic slurry, and ultimately affecting the compactness and hardness of the silicon carbide ceramic.

[0155] (6) By comparing Example 1 with Comparative Example 1, it can be seen that the sodium styrene sulfonate described in the present invention can improve the dispersibility of silicon carbide powder, so that the modified silicon carbide powder exhibits a better dispersibility in the process of preparing silicon carbide ceramics;

[0156] (7) By comparing Example 1 with Comparative Example 2, it can be seen that the sodium bisulfite in the present invention has a reducing property. Sodium bisulfite can not only adjust the free radical concentration in the obtained modifier, but also play an antioxidant role, so that the modified silicon carbide powder shows a better dispersion effect in the process of preparing silicon carbide ceramics;

[0157] (8) By comparing Example 1 with Comparative Example 3, it can be seen that the acrylic acid monomer described in the present invention will polymerize during the process of preparing the modifier, and has certain defoaming and degassing properties after polymerization. When the modified silicon carbide powder is used to prepare silicon carbide ceramics, the bubbles in the slurry can be further eliminated to form a uniform and compact embryo, thereby obtaining a silicon carbide ceramic with high hardness;

[0158] (9) By comparing Example 1 with Comparative Example 4, it can be seen that the end of the allyl polyether in the present invention contains a hydroxyl group, which can be connected to the silanol group on the surface of the silicon carbide powder through hydrogen bonding during the modification of the silicon carbide powder, thereby modifying the silicon carbide powder. At the same time, the allyl polyether also has a certain length of polyoxyethylene ether chain segments, which can effectively separate the silicon carbide powder, thereby further improving the dispersibility of the modified silicon carbide powder in the process of preparing silicon carbide ceramics;

[0159] (10) By comparing Example 1 with Comparative Example 5, it can be seen that the persulfate in the present invention is an initiator in the reaction process. The persulfate provides free radicals to initiate the reaction to obtain a modifier, so that the ceramic slurry prepared from the modified silicon carbide powder has a better dispersion effect, thereby obtaining a high-hardness silicon carbide ceramic;

[0160] (11) By comparing Example 1 with Comparative Example 6, it can be seen that the method provided by the present invention utilizes the production waste of silicon carbide crystals to prepare silicon carbide ceramics, thereby achieving the purpose of saving costs, recycling waste and protecting the environment; the method utilizes sodium styrene sulfonate, acrylic monomers and allyl polyether as raw materials, prepares a modifier under the action of a persulfate initiator, and uses the obtained modifier to perform surface modification on silicon carbide powder, thereby reducing the aggregation of the modified silicon carbide powder during the ceramic preparation process and improving the dispersion effect of the modified silicon carbide powder, and finally obtaining a modified silicon carbide slurry with lower viscosity and better dispersion, thereby obtaining silicon carbide ceramics with higher compactness and higher hardness.

[0161] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing silicon carbide ceramics from silicon carbide production waste, It is characterized in that The method comprises: (1) Pre-treating silicon carbide production waste to obtain silicon carbide powder; (2) mixing a sulfonate containing a polymerizable double bond, an acrylic acid monomer, an allyl polyether, a persulfate, a sulfite, and a first solvent to obtain a modifier; (3) modifying the silicon carbide powder obtained in step (1) with the modifier obtained in step (2) to obtain modified silicon carbide powder, and preparing silicon carbide ceramics with the modified silicon carbide powder; There is no order of precedence between step (1) and step (2).

2. The method according to claim 1, It is characterized in that The silicon carbide production waste in step (1) includes waste liquid generated during the silicon carbide crystal cutting process, split pieces generated during the silicon carbide crystal processing process, and silicon carbide powder remaining during the silicon carbide crystal growth process; Preferably, the pretreatment in step (1) includes pretreating the waste liquid generated during the silicon carbide crystal cutting process, the fragments generated during the silicon carbide crystal processing process, and the silicon carbide powder remaining during the silicon carbide crystal growth process, respectively, to obtain three pretreated silicon carbide powders, and then mixing and grinding the three pretreated silicon carbide powders to obtain silicon carbide powder.

3. The method according to claim 1 or 2, It is characterized in that The average particle size of the silicon carbide powder obtained in step (1) is less than 200 μm, preferably less than 50 μm.

4. The method according to any one of claims 1 to 3, It is characterized in that The mixing in step (2) comprises: first mixing a sulfonate containing a polymerizable double bond, a sulfite and a first solvent to obtain a first mixed material; second mixing an acrylic acid monomer and an allyl polyether to obtain a second mixed material; third mixing a persulfate and the first solvent to obtain a third mixed material; and fourth mixing the first mixed material, the second mixed material and the third mixed material, adjusting the pH and drying the mixed material to obtain a modifier; Preferably, the fourth mixing comprises: adding the second mixed material and the third mixed material to the first mixed material at a constant flow rate at 60-100° C., keeping the temperature after the addition is completed, and then cooling to 15-30° C.; Preferably, the constant flow rate is 0.1-1 ml / min; Preferably, the insulation time is 1 to 3 hours; Preferably, the pH is adjusted to 7-8.

5. The method according to claim 4, It is characterized in that In parts by weight, in the mixing process of step (2), the weight of sodium styrene sulfonate is 90 to 110 parts, the weight of sulfite is 0.21 to 2.3 parts, the weight of acrylic acid monomer is 100 to 300 parts, the weight of allyl polyether is 20 to 50 parts, and the weight of persulfate is 0.42 to 4.6 parts.

6. The method according to any one of claims 1 to 5, It is characterized in that The sulfonate containing polymerizable double bonds includes any one of sodium styrene sulfonate, sodium acrylic acid sulfonate, sodium methacrylic acid sulfonate, sodium 2-acrylamide-2-methylpropane sulfonate or sodium maleic anhydride sulfonate or a combination of at least two thereof, preferably sodium styrene sulfonate; Preferably, the acrylic monomer comprises any one of acrylic acid, methacrylic acid, methyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate or isooctyl acrylate, or a combination of at least two thereof, preferably a combination of hydroxyethyl acrylate and isooctyl acrylate; Preferably, the molecular formula of the allyl polyether is CH 2 CHCH 2 (C 2 H 4 O) m H; wherein m is 2 to 10, preferably 6 to 10.

7. The method according to any one of claims 1 to 6, It is characterized in that The modification treatment in step (3) comprises: The silicon carbide powder obtained in step (1) is mixed with the second solvent and then the pH is adjusted to obtain a primary mixture, the primary mixture is then mixed with the modifier obtained in step (2), heated to the end temperature, and then stirred while being kept warm, and a modified silicon carbide powder is obtained after solid-liquid separation; Preferably, the mass ratio of the silicon carbide powder to the second solvent is (30-50):100; Preferably, the mass ratio of the primary mixture to the modifier is 100:(0.5-1); Preferably, the pH is adjusted to 9-10 in the pH adjustment; Preferably, the end point temperature is 60-80°C; Preferably, the stirring time is 0.5 to 1 h.

8. The method according to any one of claims 1 to 7, It is characterized in that In step (3), preparing silicon carbide ceramics using the obtained modified silicon carbide powder comprises: The modified silicon carbide powder, a surfactant and a defoamer are mixed to obtain a ceramic slurry, and the obtained ceramic slurry is sintered to obtain silicon carbide ceramics; Preferably, the sintering molding comprises: injecting the obtained ceramic slurry into a mold, then performing vibration and vacuum suction in sequence to remove foam, and then performing sintering treatment; Preferably, the sintering treatment is carried out at a temperature of 2000-2400° C. and for a time of 2-6 hours.

9. The method according to any one of claims 1 to 8, It is characterized in that The method comprises: (1) The waste liquid generated during the silicon carbide crystal cutting process is sequentially graded and filtered and pickled and dried to obtain mixed particles of silicon carbide and diamond; single crystal silicon powder is added to the obtained mixed particles, and then heated to allow the single crystal silicon powder to react with the diamond in the mixed particles to generate silicon carbide, thereby obtaining a first pretreated silicon carbide powder; Crushing the fragments generated during the processing of the silicon carbide crystal to obtain a second pretreated silicon carbide powder; The silicon carbide powder remaining in the process of silicon carbide crystal growth is sequentially roasted, acid-washed and alkaline-washed to obtain a third pretreated silicon carbide powder; The first pretreated silicon carbide powder, the second pretreated silicon carbide powder and the third pretreated silicon carbide powder are mixed and then ground to obtain silicon carbide powder with an average particle size of less than 50 μm; (2) In parts by weight, a first mixture of 90 to 110 parts by weight of a sulfonate containing a polymerizable double bond, 0.21 to 2.3 parts by weight of a sulfite and 500 to 900 parts by weight of a first solvent is prepared to obtain a first mixture; a second mixture of 100 to 300 parts by weight of an acrylic acid monomer and 20 to 50 parts by weight of an allyl polyether is prepared to obtain a second mixture; a third mixture of 0.42 to 4.6 parts by weight of a persulfate and 50 to 100 parts by weight of the first solvent is prepared to obtain a third mixture; and the second mixture and the third mixture are added to the first mixture at a constant flow rate of 0.1 to 1 ml / min at 60 to 100° C., and after the addition is completed, the mixture is kept warm for 1 to 3 hours, and then cooled to 15 to 30° C., the pH is adjusted to 7 to 8, and then spray-dried to obtain a modifier; (3) mixing the silicon carbide powder obtained in step (1) and the second solvent in a mass ratio of (30-50):100, adjusting the pH to 9-10 to obtain a primary mixture, and then mixing the primary mixture with the modifier obtained in step (2) in a mass ratio of 100:(0.5-1), heating to 60-80° C., keeping the mixture warm, and stirring for 0.5-1 h, filtering, and obtaining a modified silicon carbide powder; The modified silicon carbide powder, a surfactant and a defoamer in a mass ratio of 100:(0.5-1):(0.5-1) are mixed to obtain a ceramic slurry, the obtained ceramic slurry is injected into a mold, and then vibration and vacuum suction are performed in sequence to remove foam, and then sintering treatment is performed at 2000-2400° C. for 2-6 hours to obtain silicon carbide ceramics; There is no order of precedence between step (1) and step (2).

10. A silicon carbide ceramic, It is characterized in that The silicon carbide ceramic is obtained by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of silicon carbide slurry with high solid content

    CN101830704A

  • Method for preparing silicon carbide ceramic from silicon carbide solid waste

    CN103086721A

  • Method for improving dispersion stability of silicon carbide powder in water system

    CN108314453A

  • Acrylic copolymer dispersing agent with wettability and preparation method thereof

    CN117801177A

  • Preparation method of silicon carbide ceramic

    CN117923907A