Polyurethane-coated slow-release nitrogen fertilizer with high bio-based content and application of polyurethane-coated slow-release nitrogen fertilizer in fermentation production of straw organic fertilizer
Through the combination of high-biologically based polyurethane coated sustained release nitrogen fertilizer and PTFE hydrophobic breathable membrane, the problem of long nitrogen volatility and fermentation time in straw compost is solved, the continuous supply of nitrogen and the improvement of compost quality is achieved, and environmental pollution is reduced and cost.
Patent Information
- Application Number
- CN202411133636.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the nitrogen volatility loss during straw composting is high, the fermentation time is long, and the added nitrogen retaining agent is high cost and may contain impurities, which affects the quality of the compost and soil safety.
Polyurethane enveloped sustained release nitrogen fertilizer with high biobase content is prepared by reaction of polyol, bio-isocyanate and petrochemical isocyanate, sprayed on the surface of the fertilizer core, and fermented in combination with PTFE hydrophobic and breathable membrane to achieve nitrogen Sustained release and optimization of microbial environment.
The continuous supply of nitrogen is achieved, volatilization and loss are reduced, fermentation time is shortened, the nitrogen content and quality of the compost is improved, environmental pollution is reduced, and the material is well degraded and environmentally friendly.
Smart Images

Figure CN118930386A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic fertilizers, and in particular to a polyurethane coated slow-release nitrogen fertilizer with a high bio-based content and application thereof in fermentation production of straw organic fertilizer. Background Art
[0002] As an important byproduct of agricultural production and a source of organic fertilizer, straw is rich in various nutrients and can improve soil, improve soil fertility and achieve sustainable agricultural development. It is the world's largest renewable resource. Using straw to process organic fertilizer to reasonably replace chemical fertilizers is an important means to reduce the amount of chemical fertilizers and increase their efficiency in agricultural production.
[0003] After the straw waste is crushed, it is conventionally processed into an organic fertilizer product by a composting and fermentation process. Composting and fermentation is a process in which unstable organic matter is decomposed and converted into safe and stable humus substances through the fermentation of microorganisms and a series of physical and chemical reactions by regulating parameters such as moisture, carbon-nitrogen ratio (C / N), ventilation volume, etc. Compared with other technologies, composting can effectively achieve the reduction, harmlessness and resource utilization of straw waste. However, due to the carbon-nitrogen ratio of straw being about 80, under the condition of such a high carbon-nitrogen ratio, the nitrogen element required by microorganisms is restricted, microorganisms proliferate slowly, the fermentation time is long, the humification degree of materials is low, and the fermentation is not thorough. Therefore, in the prior art, the carbon-nitrogen ratio in the composting process is reduced by increasing the application of urea, but in the heating stage of composting, a large amount of heat will be released, and a large amount of ammonia will be volatilized after urea is heated, resulting in high nitrogen volatilization loss in the early fermentation stage, and insufficient nitrogen in the late fermentation stage, which cannot guarantee the nitrogen supply of the entire fermentation process. In order to ensure the supply of nitrogen, the existing technology often slows down the volatilization loss of nitrogen by adding nitrogen retainers. However, adding too much nitrogen retainers will increase the cost of composting, especially the high price of high-quality nitrogen retainers, which will increase the economic burden of composting. Some other nitrogen retainers contain impurities or chemical substances, such as pesticide residues and heavy metals. Long-term use will affect the quality of compost products and even have a negative impact on soil and plants. Therefore, how to shorten the composting time, make fresh waste straw quickly decompose, and prepare high-quality organic fertilizer is an urgent problem to be solved in modern agricultural production. Summary of the invention
[0004] In view of the above-mentioned prior art, the object of the present invention is to provide a polyurethane coated slow-release nitrogen fertilizer with a high bio-based content and its application in the fermentation production of straw organic fertilizer.
[0005] To achieve the above object, the present invention adopts the following technical solution:
[0006] In a first aspect of the present invention, there is provided a polyurethane coated slow-release nitrogen fertilizer, comprising a fertilizer core, and a polyurethane coating material sprayed on the surface of the fertilizer core;
[0007] The polyurethane coating material is obtained by reacting polyol, bio-source isocyanate and petrochemical-source isocyanate;
[0008] The bio-source isocyanate is 1,5-pentanediisocyanate (PDI);
[0009] The petrochemical source isocyanate is one or more of polymethylene polyphenyl polyisocyanate (PAPI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and L-lysine diisocyanate (LDI).
[0010] Preferably, the petrochemical-derived isocyanate is polymethylene polyphenyl polyisocyanate (PAPI).
[0011] Preferably, the reaction conditions for preparing the polyurethane coating material are: reacting at 60-90° C. for 2-20 min.
[0012] Preferably, the mass ratio of the polyol, the bio-sourced isocyanate and the petrochemical-sourced isocyanate is 50:(15-50):(15-50)
[0013] Preferably, the polyol is one or more of soybean oil polyol, castor oil polyol, polyether polyol and polyester polyol.
[0014] The second aspect of the present invention provides a method for preparing the above-mentioned polyurethane coated slow-release nitrogen fertilizer, comprising the following steps:
[0015] The fertilizer core is heated to 60-90° C. in a coating machine, and the polyurethane coating material is pumped into the surface of the continuously moving fertilizer core in batches, with the polyurethane coating material inputted in an amount of 1-2% of the total weight of the granular fertilizer each time, and solidified for 3-6 minutes; the above steps are repeated until the polyurethane coating material accounts for 2%-5% of the total weight of the fertilizer core.
[0016] The third aspect of the present invention provides the use of the above-mentioned polyurethane coated slow-release nitrogen fertilizer in the fermentation production of straw organic fertilizer.
[0017] A fourth aspect of the present invention provides a method for producing straw organic fertilizer by fermentation, comprising the following steps:
[0018] (1) crushing straw and mixing it with livestock manure to obtain a mixed material, adding a fermentation agent and the polyurethane coated slow-release nitrogen fertilizer, mixing them evenly, piling them into a pile, and covering them with a PTFE hydrophobic breathable film for sealed fermentation;
[0019] (2) When the temperature at 22 cm from the surface of the fermentation pile reaches 50°C, turn the pile over, with an interval of 3 days between each turning. After 3 times of turning the pile over, wait for the temperature of the fermentation pile to drop below 50°C, and then let it mature and ferment under natural conditions.
[0020] Preferably, the fermentation bacteria agent is one or more of lactic acid bacteria, thermophilic actinomycetes, Bacillus, Pseudomonas, Trichoderma, white rot fungi, and Aspergillus.
[0021] Preferably, the amount of the fermentation agent added is 0.5-1.5‰ of the mass of the straw, and the number of live bacteria in the fermentation agent is ≥1×10 8 cfu / g; the addition amount of polyurethane coated slow-release nitrogen fertilizer is 3-7% of the straw mass.
[0022] Beneficial effects of the present invention:
[0023] 1. The present invention adopts low-cost, easily available and biocompatible bio-sourced isocyanates to partially replace petrochemical-derived isocyanates to prepare membrane materials with high bio-based content. Compared with petrochemical-derived materials, the membrane materials have good degradability and are more environmentally friendly. The good fluidity of 1,5-pentanediisocyanate (PDI) is utilized to improve the reaction fluidity of the coating process and reduce the agglomeration phenomenon, providing a solution to the particle adhesion and wall hanging during the production of controlled-release fertilizers. The cross-linking and interpenetrating modification of vegetable oil polyols and two curing agents can achieve 50-90 days of nitrogen sustained release without the need to add additional cross-linking agents.
[0024] 2. The present invention adopts slow-release nitrogen fertilizer fermentation to produce straw organic fertilizer to gradually release nitrogen, provide continuous nutrient supply, be beneficial to the stable and continuous activity of microorganisms, reduce the volatilization and loss of nitrogen, improve the utilization rate of nitrogen, thereby improving the nitrogen content and overall fertilizer efficiency of compost; covering the PTFE hydrophobic breathable membrane can effectively control the evaporation of water during the composting process and maintain a suitable humidity, which is beneficial to the activity of microorganisms and the normal progress of composting, maintain the temperature of the compost pile stable, promote the growth of beneficial microorganisms and the degradation of organic matter, reduce the emission of harmful gases (such as ammonia), reduce pollution to the environment, and retain more nutrients in the compost.
[0025] 3. The present invention simultaneously uses slow-release nitrogen fertilizer and PTFE hydrophobic breathable membrane to promote microbial activity, improve nutrient retention, and improve fertilizer efficiency and quality. The slow-release nitrogen fertilizer provides a stable nitrogen source, and the PTFE hydrophobic breathable membrane maintains a suitable temperature and humidity environment. The combination of the two can significantly promote the activity and reproduction of microorganisms and accelerate the decomposition of organic matter; the slow-release nitrogen fertilizer reduces nitrogen loss, and the PTFE hydrophobic breathable membrane reduces gas volatilization and water evaporation, and jointly improves the nutrient retention rate during composting; the comprehensive use of slow-release nitrogen fertilizer and PTFE hydrophobic breathable membrane can produce higher quality organic fertilizer with higher nitrogen content and better nutrient balance, thereby improving fertilizer efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 : Reaction diagram when polyurethane coated slow-release nitrogen fertilizer is prepared using Comparative Example 1, Example 2, and Comparative Example 2;
[0027] Figure 2 : Release curves of polyurethane coated slow-release nitrogen fertilizers prepared with different coating materials;
[0028] Figure 3 : Surface scanning electron microscope images of different polyurethane coated slow-release nitrogen fertilizers before and after composting (a1: surface scanning electron microscope image of the film shell of the polyurethane coated slow-release nitrogen fertilizer before composting of Comparative Example 2; a2: surface scanning electron microscope image of the film shell of the polyurethane coated slow-release nitrogen fertilizer after composting of Comparative Example 2; b1: surface scanning electron microscope image of the film shell of the polyurethane coated slow-release nitrogen fertilizer before composting of Example 2; b2: surface scanning electron microscope image of the film shell of the polyurethane coated slow-release nitrogen fertilizer after composting of Example 2; c1: surface scanning electron microscope image of the film shell of the polyurethane coated slow-release nitrogen fertilizer before composting of Comparative Example 1; c2: surface scanning electron microscope image of the film shell of the polyurethane coated slow-release nitrogen fertilizer after composting of Comparative Example 1.);
[0029] Figure 4 : Loss rates of nitrogen and urea after composting in different treatment groups;
[0030] Figure 5 : C / N during composting in different treatment groups. DETAILED DESCRIPTION
[0031] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0032] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.
[0033] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.
[0034] The strain number of the green Trichoderma used in the present invention is CICC 13029, which is purchased from the China Industrial Microbiological Culture Collection Management Center.
[0035] The activated green Trichoderma was inoculated into PDA culture medium at 10% (volume ratio), and fermented and cultured at 28° C. for 36 hours to obtain green Trichoderma fermentation liquid, which was dried to obtain green Trichoderma powder.
[0036] The PTFE hydrophobic breathable membrane used in the present invention was purchased from Maiborui Biomembrane Technology Co., Ltd.
[0037] The soybean oil polyol used in the present invention was purchased from Linyi Deken Smart Fertilizer Technology Co., Ltd.
[0038] Example 1: Preparation and composting application of polyurethane coated slow-release nitrogen fertilizer:
[0039] 1. Preparation of polyurethane coated slow-release nitrogen fertilizer:
[0040] (1) 50 g of soybean oil polyol, 15 g of polymethylene polyphenyl polyisocyanate (PAPI) and 35 g of 1,5-pentanediisocyanate (PDI) were mixed evenly and reacted at 70° C. for 10 min to obtain a polyurethane coating material;
[0041] (2) adding 10.0 kg of urea to the coating drum, setting the drum speed to 45 r / min, heating at 80±2° C. for 10 minutes to reach the preheating temperature, and spraying the polyurethane coating material evenly onto the surface of the particles for curing reaction. The input amount of the polyurethane coating material each time is 100 g, and curing is performed for 5 minutes; repeating 3 times until the polyurethane coating material accounts for 3% of the total weight of the fertilizer core, thereby obtaining a polyurethane coated slow-release nitrogen fertilizer;
[0042] 2. Composting application of polyurethane coated slow-release nitrogen fertilizer:
[0043] 1 kg of straw was crushed and 0.8 g of green Trichoderma powder (the number of viable bacteria was 1×10 8 cfu / g) and 50g polyurethane coated slow-release nitrogen fertilizer, mix well, adjust the moisture content to 55%, then pile into 1.5 meters long and 1.2 meters wide strips, cover with PTFE hydrophobic breathable membrane for sealed fermentation, when the temperature at 22cm on the surface of the fermentation pile is 50℃, turn the pile, each time the interval is 3 days, after 3 times, wait for the temperature of the fermentation pile to drop below 50℃, and then ferment under natural conditions. When the color of the pile is dark brown or black, the odor disappears and becomes lighter, and the temperature of the pile is consistent with the ambient temperature, the composting is complete. According to the test, the time required for composting is 48 days.
[0044] Example 2: Preparation and composting application of polyurethane coated slow-release nitrogen fertilizer:
[0045] 1. Preparation of polyurethane coated slow-release nitrogen fertilizer:
[0046] (1) 50 g of soybean oil polyol, 25 g of polymethylene polyphenyl polyisocyanate (PAPI) and 25 g of 1,5-pentanediisocyanate (PDI) were mixed evenly and reacted at 70° C. for 10 min to obtain a polyurethane coating material;
[0047] (2) adding 10.0 kg of urea to the coating drum, setting the drum speed to 45 r / min, heating at 80±2° C. for 10 minutes to reach the preheating temperature, and spraying the polyurethane coating material evenly onto the surface of the particles for curing reaction. The input amount of the polyurethane coating material each time is 100 g, and curing is performed for 5 minutes; repeating 3 times until the polyurethane coating material accounts for 3% of the total weight of the fertilizer core, thereby obtaining a polyurethane coated slow-release nitrogen fertilizer;
[0048] 2. Composting application of polyurethane coated slow-release nitrogen fertilizer:
[0049] 1 kg of straw was crushed and 0.8 g of green Trichoderma powder (the number of viable bacteria was 1×10 8 cfu / g) and 50g polyurethane coated slow-release nitrogen fertilizer, mix well, adjust the moisture content to 55%, then pile into 1.5 meters long and 1.2 meters wide strips, cover with PTFE hydrophobic breathable membrane for sealed fermentation, when the temperature at 22cm on the surface of the fermentation pile is 50℃, turn the pile, each time the interval is 3 days, after 3 times, wait for the temperature of the fermentation pile to drop below 50℃, and then ferment under natural conditions. When the color of the pile is dark brown or black, the odor disappears and becomes lighter, and the temperature of the pile is consistent with the ambient temperature, the composting is complete. According to the test, the time required for composting is 50 days.
[0050] Example 3: Preparation and composting application of polyurethane coated slow-release nitrogen fertilizer:
[0051] 1. Preparation of polyurethane coated slow-release nitrogen fertilizer:
[0052] (1) 50 g of soybean oil polyol, 35 g of polymethylene polyphenyl polyisocyanate (PAPI) and 15 g of 1,5-pentanediisocyanate (PDI) were mixed evenly and reacted at 70° C. for 10 min to obtain a polyurethane coating material;
[0053] (2) adding 10.0 kg of urea to the coating drum, setting the drum speed to 45 r / min, heating at 80±2° C. for 10 minutes to reach the preheating temperature, and spraying the polyurethane coating material evenly onto the surface of the particles for curing reaction. The input amount of the polyurethane coating material each time is 100 g, and curing is performed for 5 minutes; repeating 3 times until the polyurethane coating material accounts for 3% of the total weight of the fertilizer core, thereby obtaining a polyurethane coated slow-release nitrogen fertilizer;
[0054] 2. Composting application of polyurethane coated slow-release nitrogen fertilizer:
[0055] 1 kg of straw was crushed and 0.8 g of green Trichoderma powder (the number of viable bacteria was 1×10 8cfu / g) and 50g polyurethane coated slow-release nitrogen fertilizer, mix well, adjust the moisture content to 55%, then pile into 1.5 meters long and 1.2 meters wide strips, cover with PTFE hydrophobic breathable membrane for sealed fermentation, when the temperature at 22cm on the surface of the fermentation pile is 50℃, turn the pile, each time the interval is 3 days, after 3 times, wait for the temperature of the fermentation pile to drop below 50℃, and then ferment under natural conditions. When the color of the pile is dark brown or black, the odor disappears and becomes lighter, and the temperature of the pile is consistent with the ambient temperature, the composting is complete. According to the test, the time required for composting is 49 days.
[0056] Comparative Example 1:
[0057] (1) 50 g of soybean oil polyol and 50 g of 1,5-pentanediisocyanate (PDI) were mixed evenly and reacted at 70° C. for 10 min to obtain a polyurethane coating material;
[0058] (2) adding 10.0 kg of urea to the coating drum, setting the drum speed to 45 r / min, heating at 80±2° C. for 10 minutes to reach the preheating temperature, and spraying the polyurethane coating material evenly onto the surface of the particles for curing reaction. The input amount of the polyurethane coating material each time is 100 g, and curing is performed for 5 minutes; repeating 3 times until the polyurethane coating material accounts for 3% of the total weight of the fertilizer core, thereby obtaining a polyurethane coated slow-release nitrogen fertilizer;
[0059] (3) After pulverizing 1 kg of straw, add 0.8 g of green Trichoderma powder (the number of viable bacteria is 1×10 8 cfu / g) and 50g polyurethane coated slow-release nitrogen fertilizer, mix well, adjust the moisture content to 55%, then pile into 1.5 meters long and 1.2 meters wide strips, cover with PTFE hydrophobic breathable membrane for sealed fermentation, when the temperature at 22cm on the surface of the fermentation pile is 50℃, turn the pile, each time the interval is 3 days, after 3 times, wait for the temperature of the fermentation pile to drop below 50℃, and then ferment under natural conditions. When the color of the pile is dark brown or black, the odor disappears and becomes lighter, and the temperature of the pile is consistent with the ambient temperature, the composting is complete. According to the test, the time required for composting is 61 days.
[0060] Comparative Example 2:
[0061] (1) 50 g of soybean oil polyol and 50 g of polymethylene polyphenyl polyisocyanate (PAPI) were mixed evenly and reacted at 70° C. for 10 min to obtain a polyurethane coating material;
[0062] (2) adding 10.0 kg of urea to the coating drum, setting the drum speed to 45 r / min, heating at 80±2° C. for 10 minutes to reach the preheating temperature, and spraying the polyurethane coating material evenly onto the surface of the particles for curing reaction. The input amount of the polyurethane coating material each time is 100 g, and curing is performed for 5 minutes; repeating 3 times until the polyurethane coating material accounts for 3% of the total weight of the fertilizer core, thereby obtaining a polyurethane coated slow-release nitrogen fertilizer;
[0063] (3) After pulverizing 1 kg of straw, add 0.8 g of green Trichoderma powder (the number of viable bacteria is 1×10 8 cfu / g) and 50g polyurethane coated slow-release nitrogen fertilizer, mix well, adjust the moisture content to 55%, then pile into 1.5 meters long and 1.2 meters wide strips, cover with PTFE hydrophobic breathable membrane for sealed fermentation, when the temperature at 22cm on the surface of the fermentation pile is 50℃, turn the pile, each time the interval is 3 days, after 3 times, wait for the temperature of the fermentation pile to drop below 50℃, and then ferment under natural conditions. When the color of the pile is dark brown or black, the odor disappears and becomes lighter, and the temperature of the pile is consistent with the ambient temperature, the composting is complete. According to the test, the time required for composting is 51 days.
[0064] Comparative Example 3:
[0065] 1 kg of straw was crushed and 0.8 g of Trichoderma viride (the number of viable bacteria was 1 × 10 8 cfu / g) and 50g urea, mix evenly, adjust the moisture content to 55%, then pile into 1.5 meters long and 1.2 meters wide strips, cover with PTFE hydrophobic breathable membrane for sealed fermentation, and turn the pile when the temperature at 22cm on the surface of the fermentation pile is 50℃, each turning is 3 days apart, and after 3 times, wait for the temperature of the fermentation pile to drop below 50℃, and then ferment under natural conditions. When the color of the pile is dark brown or black, the odor disappears and becomes lighter, and the temperature of the pile is consistent with the ambient temperature, the composting is complete. According to the test, the time required for composting is 70 days.
[0066] Test example:
[0067] Figure 1 This is a reaction state diagram of the preparation of the polyurethane coated slow-release nitrogen fertilizer of Comparative Example 1, Example 2, and Comparative Example 2. In Comparative Example 1, the low viscosity of 1,5-pentane diisocyanate (PDI) makes the coating process smoother and without adhesion. Comparative Example 2 uses soybean oil polyol and polymethylene polyphenyl polyisocyanate (PAPI) to prepare polyurethane coated slow-release nitrogen fertilizer. Due to the high viscosity of polymethylene polyphenyl polyisocyanate (PAPI), the fertilizer sticks into agglomerates during preparation. Example 2 combines the advantages of 1,5-pentane diisocyanate (PDI) and polymethylene polyphenyl polyisocyanate (PAPI), and can also achieve a smooth reaction.
[0068] Test Example 1: Nutrient release determination:
[0069] The nitrogen release rates of the polyurethane coated slow-release nitrogen fertilizers prepared in Examples 1-3 and Comparative Examples 1-2 were measured according to the National Standard for Slow-Release Fertilizers GB / T23348-2009.
[0070] from Figure 2 It can be seen that the controlled release days of Comparative Example 1 are about 10 days, the controlled release days of Example 1 are 50 days, the controlled release days of Comparative Example 2, Examples 2 and 3 are more than 80 days, and the controlled release curves are similar, indicating that the use of bio-source isocyanate to partially replace petrochemical-source isocyanate can still achieve sustained release of nitrogen.
[0071] Test Example 2: Test on the changes of the membrane shell of polyurethane coated slow-release nitrogen fertilizer before and after composting:
[0072] The surfaces of the film shells of the polyurethane coated slow-release nitrogen fertilizers of Example 2, Comparative Example 1 and Comparative Example 2 before and after composting were observed by scanning electron microscopy.
[0073] Depend on Figure 3 It can be seen that after the composting, the membrane shells of the slow-release urea have been degraded to varying degrees, proving that the membrane shells are degradable. The membrane shell surface of Comparative Example 2 has more serious fractures and degradation, and the degradation of Comparative Example 1 is the worst. While ensuring the slow release of nitrogen, Example 2 has better degradation than Comparative Example 1.
[0074] Test Example 3: Test of organic matter content after composting in different treatment groups:
[0075] The organic matter content of the composted organic fertilizers of Examples 1-3 and Comparative Examples 1-3 was tested by potassium dichromate volumetric method. The results are shown in Table 1:
[0076] Table 1 Organic matter content after composting
[0077]
[0078] It can be seen from Table 1 that the organic matter content of the straw organic fertilizer prepared in Example 1 of the present invention is significantly higher than that of the other treatment groups.
[0079] Test Example 4: Nitrogen loss rate and carbon loss rate test of different treatment groups:
[0080] According to "Organic Fertilizer NY / T 525-2021", the total nitrogen and total organic matter contents of Examples 1-3 and Comparative Examples 1-3 were measured at the beginning of composting and after maturity, and the nitrogen loss rate and carbon loss rate were calculated by the difference between the two.
[0081] from Figure 4It can be seen that the nitrogen losses of Examples 1-3 are all below 10%, indicating that the nitrogen slow-release effect in Examples 1-3 is effective. The nitrogen losses in Comparative Examples 1 and 3 are relatively high because the slow-release effect of PDI is weak, and ordinary urea is quickly consumed and lost after being added. Although the nitrogen slow-release effect of Comparative Example 2 prepared using PAPI is similar to that of the embodiment and can also reduce nitrogen losses, PAPI is a petrochemical source material and has a greater risk of environmental pollution than biological PDI. Therefore, the combination of PDI and PAPI to prepare coated slow-release nitrogen fertilizer can not only effectively reduce nitrogen losses during composting, but also reduce the risk of environmental pollution. The carbon loss in Example 1 is only 10.1%, and the carbon losses in Examples 2, 3 and Comparative Example 2 are also controlled within 15%, indicating that coated nitrogen fertilizer can reduce carbon losses.
[0082] Test Example 5: C / N test in different composting processes:
[0083] During the composting process of Examples 1-3 and Comparative Examples 1-3, samples were taken at different time points to record the C / N ratio during the composting process. The results are as follows: Figure 5 shown.
[0084] During straw fermentation, the C / N ratio has a significant effect on the composting time and organic matter content. A higher C / N ratio (e.g., more than 30:1) usually leads to a slower composting process because excess carbon limits the growth of microorganisms, while a lower C / N ratio promotes faster composting and higher organic matter content. Optimizing the C / N ratio can effectively shorten the composting time and improve the quality of the final product.
[0085] from Figure 5 It can be seen that Example 1 can achieve the slow release of nitrogen, provide a stable nitrogen source for the entire composting process, and maintain C / N at 25±1. The PDI used in Comparative Example 1 has a poor slow release effect, and can control C / N at about 25 in the early stage, but the nitrogen is completely released on the 10th day, resulting in insufficient nitrogen supply in the subsequent period, and C / N obviously rises to about 27. In the late stage of composting, it finally stabilizes at about 25 as the fermentation proceeds. The urea used in Comparative Example 3 can also provide sufficient nitrogen in the early stage, but the lack of nitrogen in the later stage causes the C / N to rise, but as the fermentation proceeds in the later stage, the C / N rises to about 35.
[0086] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A polyurethane coated slow-release nitrogen fertilizer, It is characterized in that It includes a fertilizer core and a polyurethane coating material sprayed on the surface of the fertilizer core; The polyurethane coating material is obtained by reacting polyol, bio-source isocyanate and petrochemical-source isocyanate; The bio-source isocyanate is 1,5-pentanediisocyanate (PDI); The petrochemical source isocyanate is one or more of polymethylene polyphenyl polyisocyanate (PAPI), toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and L-lysine diisocyanate (LDI).
2. The polyurethane coated slow-release nitrogen fertilizer according to claim 1, It is characterized in that The petrochemical source isocyanate is polymethylene polyphenyl polyisocyanate (PAPI).
3. The polyurethane coated slow-release nitrogen fertilizer according to claim 1, It is characterized in that The reaction conditions for preparing the polyurethane coating material are: reacting at 60-90° C. for 2-20 minutes.
4. The polyurethane coated slow-release nitrogen fertilizer according to claim 1, It is characterized in that The mass ratio of the polyol, the bio-source isocyanate and the petrochemical-source isocyanate is 50:(15-50):(15-50).
5. The polyurethane coated slow-release nitrogen fertilizer according to claim 1, It is characterized in that The polyol is one or more of soybean oil polyol, castor oil polyol, polyether polyol and polyester polyol.
6. The method for preparing the polyurethane coated slow-release nitrogen fertilizer according to any one of claims 1 to 5, It is characterized in that The following steps are involved: The fertilizer core is heated to 60-90° C. in a coating machine, and the polyurethane coating material is pumped into the surface of the continuously moving fertilizer core in batches, wherein the input amount of the polyurethane coating material each time is 1-2% of the total weight of the granular fertilizer, and solidified for 3-6 minutes; the above steps are repeated until the polyurethane coating material accounts for 2%-5% of the total weight of the fertilizer core.
7. Use of the polyurethane coated slow-release nitrogen fertilizer according to any one of claims 1 to 5 in the fermentation production of straw organic fertilizer.
8. A method for producing straw organic fertilizer by fermentation, It is characterized in that The following steps are involved: (1) crushing the straw, adding a fermentation agent and the polyurethane coated slow-release nitrogen fertilizer according to any one of claims 1 to 5, mixing them evenly, piling them into a pile, and covering them with a PTFE hydrophobic breathable membrane for sealed fermentation; (2) When the temperature at 22 cm from the surface of the fermentation pile reaches 50°C, turn the pile over, with an interval of 3 days between each turning. After 3 times of turning the pile over, wait for the temperature of the fermentation pile to drop below 50°C, and then let it mature and ferment under natural conditions.
9. The method according to claim 8, It is characterized in that The fermentation bacteria agent is one or more of lactic acid bacteria, thermophilic actinomycetes, bacillus, pseudomonas, trichoderma, white rot fungi, and aspergillus.
10. The method according to claim 9, It is characterized in that The amount of the fermentation agent added is 0.5-1.5‰ of the mass of the straw, and the number of live bacteria in the fermentation agent is ≥1×10 8 cfu / g; the addition amount of polyurethane coated slow-release nitrogen fertilizer is 3-7% of the straw mass.
Citation Information
Cited By
Crushed particle controlled-release organic fertilizer as well as preparation method and application thereof
CN122127178A