Preparation method of lithium iron manganese phosphate positive electrode material precursor

By using the preparation method of Mn0.6Fe0.4C2O4·2H2O in the precursor of lithium manganese iron phosphate positive electrode material, the problem of uneven distribution of transition metal elements is solved, the high energy density and cycle stability of the material are achieved, and the process is simplified. Suitable for industrial production.

CN118930429APending Publication Date: 2024-11-12FUDAN UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410925886.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing co-precipitation method to prepare transition metal elements in the precursor of lithium manganese iron phosphate positive electrode material is unevenly distributed, resulting in poor electrochemical performance and cannot meet the needs of high energy density and cycling stability.

Method used

Mn0.6Fe0.4C2O4·2H2O is used as the precursor of lithium manganese iron phosphate positive electrode material. By dissolving the manganese source and iron source in proportion, adding the oxalate system for dropwise addition and mixing, controlling the pH value and reaction temperature, and using antioxidants. Filtration, washing and freeze-drying to achieve atomic level uniform mixing of manganese and iron.

Benefits of technology

The controllable distribution of the ratio of manganese and ferromanganese is achieved, the electrochemical performance and cycle stability of the material are improved, the preparation process is simplified, and it is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930429A_ABST
    Figure CN118930429A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of material design, and particularly relates to a preparation method of a lithium iron manganese phosphate positive electrode material precursor of a lithium ion battery. The method comprises the following steps: preparing divalent manganese and divalent iron ions into a mixed solution under the protection of an inert atmosphere or an antioxidant, mixing the mixed solution with a solution containing oxalate ions, and controlling the reaction temperature, pH and stirring rate; and filtering, washing and freeze-drying the ferro-manganese obtained by coprecipitation in sequence to finally obtain the ferro-manganese oxalate precursor. The prepared oxalate ferromanganese precursor is good in consistency, the element proportion meets the requirement, and metal ions are evenly distributed. The method is low in cost and simple in process, can be used for large-scale production, and has good economic benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to a method for preparing a lithium manganese iron phosphate positive electrode material precursor. Background Art

[0002] The power battery industry is driving new energy vehicles forward. Ternary lithium batteries and lithium iron phosphate batteries have long been divided into two markets. With the decline of policy subsidies and technological breakthroughs, the cost-effectiveness of lithium iron phosphate has become more prominent (low price, abundant output, long service life and good thermal stability). Power battery manufacturers prefer lithium iron phosphate, and the installed capacity of lithium iron phosphate batteries has surpassed ternary cathode materials to top the list.

[0003] However, LiFePO 4 (LFP) Because the specific capacity is close to the theoretical value and the operating voltage is only 3.4V, the energy density is close to the "ceiling", which makes it difficult to meet the increasingly high requirements of power batteries in terms of energy density, limiting the further development of lithium iron phosphate batteries. 4 Compared with LFP, LMP has weaker cycle stability, but the voltage platform is as high as 4.1V, the self-discharge rate is low, the material is mature, the cost is low, and the energy density is higher than LFP. At this time, the synergistic effect of Mn and Fe is used, that is, Mn is added to LFP to form a lithium iron manganese phosphate solid solution, which combines the advantages of LFP (stable electrochemical performance and high safety) and LMP (high voltage). x Fe 1-x PO 4 (LMFP) came into being, which can improve the voltage platform while maintaining the stability of lithium iron phosphate. Under the condition that the theoretical capacity is 170mAh / g, the theoretical energy density is 20% higher than that of lithium iron phosphate.

[0004] At present, the methods for preparing lithium manganese iron phosphate include solid phase method, water (solvent) thermal method, sol-gel method, co-precipitation method, etc. The solid phase method has a simple process but a long synthesis time, and it is not easy to control the particle size and morphology of the product. The water (solvent) thermal method can control the size and morphology of the particles, and the size is uniform, but the experimental conditions are harsh and need to be carried out under high temperature and high pressure conditions, which is not conducive to large-scale industrial production. The material prepared by the sol-gel method has uniform and fine particle size, less agglomeration, simple preparation process, and less energy consumption. However, its production cycle is long and cannot meet the needs of rapid industrial production. The co-precipitation method has a simple process, low equipment requirements, and is easy to mass produce. It is a good preparation method for preparing lithium manganese iron phosphate positive electrode materials. However, the oxidation precursors and phosphate precursors currently prepared have a large order of magnitude difference in the precipitation solubility product constants formed by Mn and Fe with other salts, resulting in uneven distribution of the precursor manganese iron, and cannot achieve good mixing at the atomic level, resulting in poor cyclicity of the lithium manganese iron phosphate material obtained by adding lithium source and phosphorus source, and unable to exert electrochemical performance. Summary of the invention

[0005] The present invention aims to provide a lithium manganese iron phosphate positive electrode material precursor Mn 0.6 Fe 0.4 C 2 O 4 ·2H 2 The preparation method of O can achieve atomic-level mixing of transition metals, simplify the preparation process of lithium manganese iron phosphate positive electrode materials, and solve the problem of uneven distribution of transition metal elements in the precursor of lithium manganese iron phosphate positive electrode materials prepared by the existing co-precipitation method, which leads to poor electrochemical performance.

[0006] The lithium manganese iron phosphate positive electrode material precursor Mn 0.6 Fe 0.4 C 2 O 4 ·2H 2 The preparation method of O, the specific steps are as follows:

[0007] (1) dissolving a manganese source and an iron source in a required ratio to prepare a mixed solution I;

[0008] (2) preparing a compound providing oxalate ions into solution II;

[0009] (3) adding the two solutions of step (1) and step (2) dropwise and mixing;

[0010] (4) adding an antioxidant to the solution;

[0011] (5) controlling the pH value of the solution to 1-5, the dropwise acceleration rate to 0.5-5 mL / min, the reaction temperature to 30-80° C., and the reaction time to 4-12 h;

[0012] (6) Filter, wash, and freeze-dry to obtain the ferromanganese oxalate precursor Mn 0.6 Fe 0.4 C 2 O 4 ·2H 2 O powder.

[0013] In step (1) of the present invention, the manganese source used is a divalent manganese source, specifically at least one of manganese sulfate, manganese nitrate, manganese carbonate and manganese chloride. Preferably, the divalent manganese source is manganese sulfate.

[0014] In step (1) of the present invention, the iron source used is a divalent iron source, specifically at least one of ferrous sulfate and ferrous chloride, and preferably the divalent iron source is ferrous sulfate.

[0015] In step (2) of the present invention, the compound providing the oxalate ion is at least one of oxalic acid, ammonium oxalate and sodium oxalate, and preferably the compound providing the oxalate ion is ammonium oxalate.

[0016] In step (3) of the present invention, the mixing method is one of the following three methods: solution I is added dropwise to solution II, solution II is added dropwise to solution I, and deionized water is added dropwise to solution I and solution II simultaneously. The preferred mixing method is that deionized water is added dropwise to solution I and solution II simultaneously.

[0017] In step (4) of the present invention, the antioxidant is at least one of ascorbic acid, citric acid, butylated hydroxyanisole and butylated hydroxytoluene, and preferably the antioxidant is ascorbic acid.

[0018] In step (5) of the present invention, the pH is preferably 1-3.

[0019] In step (5) of the present invention, the reaction temperature is preferably 50-65°C, more preferably 60°C.

[0020] In step (5) of the present invention, the dropping rate is preferably 0.5 to 3 mL / min, and more preferably 0.5 to 1 mL / min.

[0021] In step (5) of the present invention, the preferred reaction time is 4 to 8 hours.

[0022] Advantages of the present invention:

[0023] The present invention utilizes that divalent iron ions and divalent manganese ions have similar precipitation coefficients in the oxalate system, and the solubility product constant is in the same order of magnitude, so that the oxalate system is used for co-precipitation, and the two transition metal elements of manganese and iron can be uniformly mixed at the atomic level, the manganese-iron ratio can be controlled, and the distribution inside the material lattice is uniform, and the morphology and particle size of the precursor are controllable. The method has a simple synthesis process, easy to obtain raw materials and low cost, low equipment requirements, and is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 is the XRD diffraction pattern of the final product in Example 1.

[0025] Figure 2 is a SEM image of the final product in Example 1.

[0026] Figure 3 It is the XRD diffraction pattern of the final product in Example 2.

[0027] Figure 4 is the SEM image of the final product in Example 2. DETAILED DESCRIPTION

[0028] The following are specific embodiments of the present invention, and the present invention is further described by combining the specific embodiments with the accompanying drawings. It is worth noting that the following embodiments are provided to better describe and understand the present invention, and are not limited to the best implementation mode, and do not limit the content and protection scope of the present invention. Any changes or equivalent substitutions that do not deviate from the concept of the present invention are included in the protection scope of the present invention.

[0029] Example 1, ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 Preparation of O.

[0030] (1) Take 2.5355 g MnSO 4 ·H 2 O, 2.7815 g FeSO 4 7H 2 O and 0.5g ascorbic acid are placed in a beaker, 50mL of deionized water is added, and ultrasonic stirring is performed to dissolve the mixed solution, wherein the concentration of divalent manganese ions in the mixed solution is 0.3mol / L, the concentration of divalent iron ions is 0.2mol / L, and the ratio of manganese to iron is 6:4.

[0031] (2) Take 4.2637 g (NH 4 ) 2 C 2 O 4 ·H 2 O was placed in a beaker, 50 mL of deionized water was added, and ultrasonic stirring was performed to dissolve it to obtain a 0.6 mol / L ammonium oxalate solution.

[0032] (3) The solutions in step (1) and step (2) are mixed by a dropwise method, with deionized water as the third base liquid, and the dropwise acceleration rates of the two solutions are controlled to be consistent so that they are added to the reactor at the same rate. 2 Carry out under inert atmosphere.

[0033] (4) The reaction temperature in step (3) was controlled to be 60° C., the dropwise acceleration rate was 0.5 mL / min, the reaction time was 8 h, and the pH value of the solution was adjusted to 3 using 1 mol / L sulfuric acid and 25 wt % ammonia water.

[0034] (5) After the reaction is completed, the mixture is filtered and washed with deionized water at 60°C, and then freeze-dried for 12 hours to obtain the ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 O powder.

[0035] Example 2, ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 Preparation of O

[0036] (1) Take 2.5355 g MnSO 4 ·H 2 O, 2.7815 g FeSO 4 7H 2 O and 0.5g ascorbic acid are placed in a beaker, 50mL of deionized water is added, and ultrasonic stirring is performed to dissolve the mixed solution, wherein the concentration of divalent manganese ions in the mixed solution is 0.3mol / L, the concentration of divalent iron ions is 0.2mol / L, and the ratio of manganese to iron is 6:4.

[0037] (2) Take 4.2637 g (NH 4 ) 2 C 2 O 4 ·H 2 O was placed in a beaker, 50 mL of deionized water was added, and ultrasonic stirring was performed to dissolve it to obtain a 0.6 mol / L ammonium oxalate solution.

[0038] (3) The solutions in step (1) and step (2) are mixed by a dropwise method, with deionized water as the third base liquid, and the dropwise acceleration rates of the two solutions are controlled to be consistent so that they are added to the reactor at the same rate. 2 Carry out under inert atmosphere.

[0039] (4) The reaction temperature in step (3) was controlled to be 60° C., the dropwise acceleration rate was 0.5 mL / min, the reaction time was 8 h, and the pH value of the solution was adjusted to 2 using 1 mol / L sulfuric acid and 25 wt % ammonia water.

[0040] (5) After the reaction is completed, the mixture is filtered and washed with deionized water at 60°C, and then freeze-dried for 12 hours to obtain the ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 O powder.

[0041] Example 3, ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 Preparation of O

[0042] (1) Take 2.5355 g MnSO 4 ·H 2 O, 2.7815 g FeSO 4 7H 2 O and 0.5g ascorbic acid are placed in a beaker, 50mL of deionized water is added, and ultrasonic stirring is performed to dissolve the mixed solution, wherein the concentration of divalent manganese ions in the mixed solution is 0.3mol / L, the concentration of divalent iron ions is 0.2mol / L, and the ratio of manganese to iron is 6:4.

[0043] (2) Take 4.2637 g (NH 4 ) 2 C 2 O 4 ·H 2 O was placed in a beaker, 50 mL of deionized water was added, and ultrasonic stirring was performed to dissolve it to obtain a 0.6 mol / L ammonium oxalate solution.

[0044] (3) The solutions in step (1) and step (2) are mixed by a dropwise method, with deionized water as the third base liquid, and the dropwise acceleration rates of the two solutions are controlled to be consistent so that they are added to the reactor at the same rate. 2 Carry out under inert atmosphere.

[0045] (4) The reaction temperature in step (3) was controlled to be 60° C., the dropwise acceleration rate was 0.5 mL / min, the reaction time was 8 h, and the pH value of the solution was adjusted to 4 using 1 mol / L sulfuric acid and 25 wt % ammonia water.

[0046] (5) After the reaction is completed, the mixture is filtered and washed with deionized water at 60°C, and then freeze-dried for 12 hours to obtain the ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 O powder.

[0047] Example 4, ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 Preparation of O

[0048] (1) Take 2.5355 g MnSO 4 ·H 2 O, 2.7815 g FeSO 4 7H 2 O and 0.5g ascorbic acid are placed in a beaker, 50mL of deionized water is added, and ultrasonic stirring is performed to dissolve the mixed solution, wherein the concentration of divalent manganese ions in the mixed solution is 0.3mol / L, the concentration of divalent iron ions is 0.2mol / L, and the ratio of manganese to iron is 6:4.

[0049] (2) Take 4.2637 g (NH 4 ) 2 C 2 O 4 ·H 2 O was placed in a beaker, 50 mL of deionized water was added, and ultrasonic stirring was performed to dissolve it to obtain a 0.6 mol / L ammonium oxalate solution.

[0050] (3) The solutions in step (1) and step (2) are mixed by a dropwise method, with deionized water as the third base liquid, and the dropwise acceleration rates of the two solutions are controlled to be consistent so that they are added to the reactor at the same rate. 2 Carry out under inert atmosphere.

[0051] (4) The reaction temperature in step (3) was controlled to be 80° C., the dropwise acceleration rate was 0.5 mL / min, the reaction time was 8 h, and the pH value of the solution was adjusted to 3 using 1 mol / L sulfuric acid and 25 wt % ammonia water.

[0052] (5) After the reaction is completed, the mixture is filtered and washed with deionized water at 60°C, and then freeze-dried for 12 hours to obtain the ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 O powder.

[0053] Example 5, ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 Preparation of O

[0054] (1) Take 2.5355 g MnSO 4 ·H2 O, 2.7815 g FeSO 4 7H 2 O and 0.5g ascorbic acid are placed in a beaker, 50mL of deionized water is added, and ultrasonic stirring is performed to dissolve the mixed solution, wherein the concentration of divalent manganese ions in the mixed solution is 0.3mol / L, the concentration of divalent iron ions is 0.2mol / L, and the ratio of manganese to iron is 6:4.

[0055] (2) Take 4.2637 g (NH 4 ) 2 C 2 O 4 ·H 2 O was placed in a beaker, 50 mL of deionized water was added, and ultrasonic stirring was performed to dissolve it to obtain a 0.6 mol / L ammonium oxalate solution.

[0056] (3) adding the ferromanganese mixed solution in step (1) dropwise to the ammonium oxalate solution in step (2), and reacting at N 2 Carry out under inert atmosphere.

[0057] (4) The reaction temperature in step (3) was controlled to be 60° C., the dropwise acceleration rate was 0.5 mL / min, the reaction time was 8 h, and the pH value of the solution was adjusted to 3 using 1 mol / L sulfuric acid and 25 wt % ammonia water.

[0058] (5) After the reaction is completed, the mixture is filtered and washed with deionized water at 60°C, and then freeze-dried for 12 hours to obtain the ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 O powder.

[0059] Example 6, ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 Preparation of O

[0060] (1) Take 2.5355 g MnSO 4 ·H 2 O, 2.7815 g FeSO 4 7H 2 O and 0.5g ascorbic acid are placed in a beaker, 50mL of deionized water is added, and ultrasonic stirring is performed to dissolve the mixed solution, wherein the concentration of divalent manganese ions in the mixed solution is 0.3mol / L, the concentration of divalent iron ions is 0.2mol / L, and the ratio of manganese to iron is 6:4.

[0061] (2) Take 4.2637 g (NH 4 )2 C 2 O 4 ·H 2 O was placed in a beaker, 50 mL of deionized water was added, and ultrasonic stirring was performed to dissolve it to obtain a 0.6 mol / L ammonium oxalate solution.

[0062] (3) adding the ammonium oxalate solution in step (2) dropwise to the ferromanganese mixed solution in step (1), reacting at N 2 Carry out under inert atmosphere.

[0063] (4) The reaction temperature in step (3) was controlled to be 60° C., the dropwise acceleration rate was 0.5 mL / min, the reaction time was 8 h, and the pH value of the solution was adjusted to 3 using 1 mol / L sulfuric acid and 25 wt % ammonia water.

[0064] (5) After the reaction is completed, the mixture is filtered and washed with deionized water at 60°C, and then freeze-dried for 12 hours to obtain the ferromanganese oxalate precursor Fe 0.4 Mn 0.6 C 2 O 4 ·2H 2 O powder.

[0065] The ferromanganese oxalate prepared in the above example was used to prepare a lithium ion battery according to the following method:

[0066] (1) Preparation of lithium manganese iron phosphate positive electrode material

[0067] The ferromanganese oxalate precursor prepared in the above examples and lithium dihydrogen phosphate were mixed in a molar ratio of Li: (Mn + Fe) = 1:1, and then 8 wt% of glucose was added for ball milling. After that, the mixture was calcined at 500 ° C for 4 h and 660 ° C for 10 h under a nitrogen atmosphere, with a heating rate of 2 ° C / min -1 , and obtain the LFMP@C sample.

[0068] (2) Preparation of positive electrode sheets and assembly of batteries

[0069] The positive electrode is composed of 90wt% LFMP, 5wt% Super P and 5wt% PVDF. The above materials are dispersed in NMP solvent and stirred to form a uniform slurry. Then it is evenly coated on aluminum foil and vacuum dried at 80°C for 12h. The dried electrode is cut into small discs with a diameter of 12mm as the positive electrode. In order to test the electrochemical properties of the material, LFMP is used as the positive electrode, lithium is used as the negative electrode, CESI 005 model is used as the electrolyte, PP microporous membrane is used as the separator, and CR2016 type batteries are assembled in an argon-filled glove box. Constant current charge and discharge tests (1C=170mA g) were carried out at different current densities, the voltage range is 2.5-4.5V, and the temperature is 25°C. -1 The prepared battery was first left to stand for 12 h, then activated at 0.1C for three cycles, and then cycled at 1C for 100 cycles. The test results are shown in Table 1.

[0070] Table 1 Test results of button batteries

[0071] <![CDATA[Initial discharge specific capacity / mAh g -1 > Example 1 159.8 Example 2 160.5 Example 3 157.3 Example 4 156.4 Example 5 155.9 Example 6 155.6 .

[0072] The above embodiments describe the basic principles, main features and advantages of the present invention, which are merely examples for the purpose of clarifying the description, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A lithium manganese iron phosphate cathode material precursor Mn 0.6 Fe 0.4 The method for preparing C2O4·2H2O is characterized in that: The specific steps are as follows: (1) dissolving a manganese source and an iron source in a required ratio to prepare a mixed solution I; (2) preparing a compound providing oxalate ions into solution II; (3) adding the two solutions of step (1) and step (2) dropwise and mixing; (4) adding an antioxidant to the solution; (5) controlling the pH value of the solution to 1-5, the dropwise acceleration rate to 0.5-5 mL / min, the reaction temperature to 30-80° C., and the reaction time to 4-12 h; (6) Filter, wash, and freeze-dry to obtain the ferromanganese oxalate precursor Mn 0.6 Fe 0.4 C2O4·2H2O powder.

2. The preparation method according to claim 1, characterized in that: The manganese source in step (1) is a divalent manganese source, specifically selected from manganese sulfate, manganese nitrate, manganese carbonate and manganese chloride.

3. The preparation method according to claim 1, characterized in that: The iron source in step (1) is a divalent iron source, specifically selected from ferrous sulfate and ferrous chloride.

4. The preparation method according to claim 1, characterized in that: The oxalate ion compound in step (2) is selected from oxalic acid, ammonium oxalate and sodium oxalate.

5. The preparation method according to claim 1, characterized in that: The mixing method in step (3) is that solution I is added dropwise to solution II, solution II is added dropwise to solution I, or solution I and solution II are simultaneously added dropwise to deionized water.

6. The preparation method according to claim 1, characterized in that: The antioxidant in step (4) is selected from ascorbic acid, citric acid, butylated hydroxyanisole, and butylated hydroxytoluene.

Citation Information

Cited By

  • Production equipment and production method of lithium iron manganese phosphate positive electrode material precursor

    CN119500014A