Preparation method of high-purity hydroxyethyl acrylate
By using zeolite molecular sieve particles with specific pore structures and vanadate-impregnated zeolite-based catalysts in the synthesis of hydroxyethyl acrylate, the safety and by-product problems of catalysts in the prior art are solved, yield and purity are improved, and purity is reduced. The use of binder achieves an efficient and safe catalytic effect.
Patent Information
- Application Number
- CN202411116691.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, chromium-based catalysts have safety hazards. Iron-based catalysts lead to more by-products, affecting the yield and purity of hydroxyethyl acrylate. In addition, the extremely fine powder form of magnetic zeolite molecular sieve requires the addition of a large amount of binder to process, reducing the performance of the catalyst. .
Tetrapropyl ammonium hydroxide, silica sol and aluminum sol are used to form zeolite molecular sieve particles with specific pore structures during the crystallization process, and vanadium ions are impregnated in the vanadate solution to form a new active center for catalyzing acrylic acid and Condensation reaction of ethylene oxide reduces side reactions and improves product desorption efficiency.
Improves the yield and purity of hydroxyethyl acrylate, avoids the reduction of the performance of the binder on the catalyst, provides a high mechanical strength zeolite-based catalyst, no or only a small amount of binder is required, and the raw materials used are non-toxic or low-toxic. Have economic benefits.
Smart Images

Figure CN118930430A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hydroxyalkyl acrylate series products, and in particular to a method for preparing high-purity hydroxyethyl acrylate. Background Art
[0002] 2-Hydroxyethyl acrylate (HEA) is a colorless, transparent liquid with a carbon-carbon double bond and two functional groups, a hydroxyl group. It can participate in a variety of chemical reactions and has a wide range of application values in many industrial fields such as fiber processing and coatings industry. The CAS number of 2-Hydroxyethyl acrylate is 818-61-1, the melting point is -60°C, the boiling point is 210-215°C (1.6kPa), the relative density is 1.1098 (20 / 4°C), the refractive index is 1.449-1.451, and the viscosity is 5.34mPa·s (25°C). In industrial production, HEA is mainly prepared by the addition reaction of acrylic acid and ethylene oxide in the presence of a catalyst and an inhibitor. Commonly used catalysts include chromium catalysts, iron catalysts, etc. The synthesis process of HEA is mature and diverse, including direct esterification, ring-opening reaction, ester exchange, etc. Among them, the ring-opening reaction method has become the main method of industrial production due to its advantages such as fast reaction, high conversion rate and simple post-processing.
[0003] In the prior art, chromium-based catalysts are generally highly toxic and pose certain safety hazards; iron-based catalysts will result in more by-products, which in turn affects the yield and purity. The invention patent with patent publication number CN103288639A discloses a method for synthesizing hydroxyethyl acrylate, using a magnetic zeolite molecular sieve as a catalyst. The magnetic zeolite molecular sieve is a magnetic 4A zeolite molecular sieve, but the molecular sieve prepared by this method is in the form of an extremely fine powder, usually only a few microns in size, which is extremely inconvenient to use in industry. Therefore, it must be processed into aggregates with a certain shape and size. The solution is to add 20-60% of a binder, but the addition of a binder will correspondingly reduce the various properties of the zeolite molecular sieve, reduce its activity and selectivity, and thus affect the synthesis efficiency and product quality of hydroxyethyl acrylate. Summary of the invention
[0004] In order to solve the problems mentioned in the above background technology, the present invention provides a method for preparing high-purity hydroxyethyl acrylate.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing high-purity hydroxyethyl acrylate comprises the following steps:
[0007] S1, adding acrylic acid and zeolite-based catalyst into a condensation reaction kettle, stirring and heating with steam, slowly introducing ethylene oxide into the reaction kettle through the liquid, controlling the reaction temperature, and keeping the temperature to react to obtain a crude product;
[0008] S2, adding the crude product to a distillation kettle, adding a polymerization inhibitor, distilling under reduced pressure, heating with steam, and in continuous production, the distillation is terminated when the liquid level of the reaction liquid in the intermediate kettle is lower than the liquid level gauge, collecting the product, and obtaining a hydroxyethyl acrylate finished product and a distillation residue;
[0009] S3. The distillation residue enters the thin film evaporator again, is heated by steam, and the product is collected to obtain the hydroxyethyl acrylate finished product and distillation residue, which is then concentrated for solid waste treatment.
[0010] The chemical equation for the reaction is:
[0011]
[0012] Furthermore, in step S1, the temperature of steam heating is 75-80°C, the stirring speed is 100-200 rpm, and after the introduction of ethylene oxide, the reaction temperature is controlled at 85-95°C, and the insulation time is 30-60 min.
[0013] Furthermore, in step S2, the pressure of the reduced pressure distillation is 0.1-0.5 MPa, and the temperature of the steam heating is 100-110°C.
[0014] Furthermore, the temperature of steam heating in step S3 is 92-100°C.
[0015] Furthermore, the mass ratio of acrylic acid, ethylene oxide, zeolite-based catalyst and polymerization inhibitor is 2000:(1300-1400):(15-20):(0.9-1), and the polymerization inhibitor is 2,2,6,6-tetramethylpiperidinoxide.
[0016] Furthermore, the zeolite-based catalyst in step S1 is prepared by the following steps:
[0017] A1. Add tetrapropylammonium hydroxide to deionized water, adjust the pH value to 10-11 with sodium hydroxide, add silica sol and aluminum sol under continuous stirring, transfer to an autoclave with a polytetrafluoroethylene liner, seal, put in an oven for crystallization, cool to room temperature, filter, wash with deionized water until the washing liquid is neutral, and dry at 80-100°C to constant weight to obtain zeolite molecular sieve particles;
[0018] A2, adding vanadate powder to deionized water, heating to 80-90° C., to prepare a 0.1-0.5 mol / L vanadate solution;
[0019] A3. Add zeolite molecular sieve particles into vanadate solution and immerse for 2-3 hours, filter, wash with deionized water until the washing liquid is clear and transparent, and then place in a muffle furnace for solidification to obtain a zeolite-based catalyst.
[0020] Furthermore, in step A1, the mass ratio of tetrapropylammonium hydroxide, deionized water, silica sol and aluminum sol is (5-7):50:(25-30):(1-1.5).
[0021] Furthermore, in step A1, the crystallization temperature is 170-180° C., and the crystallization time is 48-72 h.
[0022] Furthermore, in step A2, the vanadate is an orthovanadate, including one of sodium vanadate, potassium vanadate, bismuth vanadate, strontium vanadate, sodium ammonium vanadate, calcium vanadate, magnesium vanadate, and indium vanadate.
[0023] Furthermore, in step A3, the mass ratio of the zeolite molecular sieve particles to the vanadate solution is (8-15):(20-26), and slight stirring may be performed during the impregnation, with the stirring speed not exceeding 50 rpm.
[0024] Furthermore, in step A3, the curing temperature is 600-700° C., and the curing time is 1-2 hours.
[0025] Furthermore, the preparation method of the silica sol in step A1 is: sodium silicate is used as a silicon source, sodium silicate is added to deionized water, the mass ratio of sodium silicate to deionized water is (25-30):50, heating to 60-70°C and continuing until the sodium silicate is completely dissolved, adjusting the pH value to 9-10 with dilute hydrochloric acid, and standing and aging at room temperature for 24-48 hours.
[0026] Furthermore, the preparation method of the aluminum sol in step A1 is: aluminum salt is used as an aluminum source, preferably, the aluminum salt is aluminum sulfate, the aluminum salt is added to deionized water, the mass ratio of the aluminum salt to deionized water is (1-1.5):50, heated to 60-70°C and continuously stirred until the aluminum salt is completely dissolved, the pH value is adjusted to 6-7 with a dilute sodium hydroxide solution, and allowed to stand and age at room temperature for 24-48 hours.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. In this technical solution, with tetrapropylammonium hydroxide (TPAOH) as a template, silica sol and aluminum sol form zeolite molecular sieve particles with a pore structure of straight cylindrical pores and "Z"-shaped transverse pores during the crystallization process, which provides abundant active sites and is also conducive to the diffusion of reactant molecules and the desorption of products. Reactant molecules (small molecules such as acrylic acid and ethylene oxide) can more easily enter the interior of the pores and fully contact the active sites, thereby improving the catalytic efficiency. The zeolite molecular sieve particles are immersed in a vanadate solution, and vanadium ions are allowed to enter the pores of the zeolite molecular sieve to form new active centers. In this process, vanadium ions replace some ions in the zeolite molecular sieve framework, or interact with groups such as hydroxyl groups on the framework, thereby changing the local microstructure of the zeolite molecular sieve, which can be conducive to the adsorption and activation of reactant molecules, as well as the rapid desorption of products. Compared with traditional chromium or iron catalysts, zeolite-based catalysts can more accurately control the reaction path, reduce the occurrence of side reactions, and thus increase the yield and purity of the target product hydroxyethyl acrylate.
[0029] 2. The magnetic 4A zeolite molecular sieve in the prior art is in the form of an extremely fine powder, lacking effective bonding force between particles, and having low mechanical strength. It is necessary to add a large amount of binder for processing before use. Adding a large amount of binder will partially block the pores of the zeolite molecular sieve, reduce the exposure of active sites, and thus reduce the activity and selectivity of the catalyst. In addition, the binder itself may not have catalytic activity, and may even introduce inert components, further reducing the performance of the catalyst. The structure of the zeolite-based catalyst particles in the present invention is more compact, and the bonding force between particles is enhanced, so it has a higher mechanical strength, and can be used directly without or with only a small amount of binder, thereby avoiding the reduction of the catalyst performance by the binder.
[0030] 3. In this technical solution, the raw materials used for the zeolite-based catalyst are non-toxic or low-toxic, and can be recycled and reused after washing and drying, which has certain economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 It is a flowchart of the steps of the present invention;
[0033] Figure 2 It is a feed flow chart of the present invention. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Unless otherwise specified, the raw materials used in the present invention are all conventional products purchased from the market, and the GC of acrylic acid is ≥99%.
[0036] Preparation Example 1
[0037] Preparation of silica sol: add 25 kg sodium silicate into 50 kg deionized water, heat to 60°C and continue until the sodium silicate is completely dissolved, adjust the pH value to 9 with dilute hydrochloric acid, and let stand at room temperature for 24 hours;
[0038] Preparation of aluminum sol: Add 1 kg aluminum sulfate into 50 kg deionized water, heat to 60°C and continue stirring until the aluminum salt is completely dissolved, adjust the pH value to 6 with dilute sodium hydroxide solution, and let stand at room temperature for 24 hours.
[0039] Preparation Example 2
[0040] The zeolite-based catalyst is prepared by the following steps:
[0041] A1. Add 5 kg of tetrapropylammonium hydroxide to 50 kg of deionized water, adjust the pH value to 10 with sodium hydroxide, add 25 kg of the silica sol prepared in Preparation Example 1 and 1 kg of the aluminum sol prepared in Preparation Example 1 under continuous stirring, transfer to an autoclave with a polytetrafluoroethylene liner, seal, place in an oven at 170° C. for crystallization for 48 h, cool to room temperature, filter, wash with deionized water until the washing liquid is neutral, and dry at 80° C. to constant weight to obtain zeolite molecular sieve particles;
[0042] A2, adding sodium vanadate powder to deionized water, heating to 80°C, to prepare a 0.1 mol / L sodium vanadate solution;
[0043] A3. Add 8 kg of zeolite molecular sieve particles into 20 kg of sodium vanadate solution and immerse for 2 hours, filter, wash with deionized water until the washing liquid is clear and transparent, and then place in a muffle furnace and cure at 600° C. for 1 hour to obtain a zeolite-based catalyst.
[0044] Preparation Example 3
[0045] The zeolite-based catalyst is prepared by the following steps:
[0046] A1. Add 6 kg of tetrapropylammonium hydroxide to 50 kg of deionized water, adjust the pH value to 10 with sodium hydroxide, add 27 kg of the silica sol prepared in Preparation Example 1 and 1.3 kg of the aluminum sol prepared in Preparation Example 1 under continuous stirring, transfer to an autoclave with a polytetrafluoroethylene liner, seal, place in an oven at 175° C. for crystallization for 60 h, cool to room temperature, filter, wash with deionized water until the washing liquid is neutral, and dry at 90° C. to constant weight to obtain zeolite molecular sieve particles;
[0047] A2, adding sodium vanadate powder into deionized water, heating to 85°C, to prepare a 0.3 mol / L sodium vanadate solution;
[0048] A3. Add 10 kg of zeolite molecular sieve particles into 23 kg of sodium vanadate solution and immerse for 2.5 hours, filter, wash with deionized water until the washing liquid is clear and transparent, and then place in a muffle furnace and cure at 650° C. for 1.5 hours to obtain a zeolite-based catalyst.
[0049] Preparation Example 4
[0050] The zeolite-based catalyst is prepared by the following steps:
[0051] A1. Add 7 kg of tetrapropylammonium hydroxide to 50 kg of deionized water, adjust the pH value to 11 with sodium hydroxide, add 30 kg of the silica sol prepared in Preparation Example 1 and 1.5 kg of the aluminum sol prepared in Preparation Example 1 under continuous stirring, transfer to an autoclave with a polytetrafluoroethylene liner, seal, place in an oven at 180° C. for crystallization for 72 h, cool to room temperature, filter, wash with deionized water until the washing liquid is neutral, and dry at 100° C. to constant weight to obtain zeolite molecular sieve particles;
[0052] A2, adding sodium vanadate powder to deionized water, heating to 90° C., to prepare a 0.5 mol / L sodium vanadate solution;
[0053] A3. Add 15 kg of zeolite molecular sieve particles into 26 kg of sodium vanadate solution and immerse for 3 hours, filter, wash with deionized water until the washing liquid is clear and transparent, and then place in a muffle furnace and cure at 700° C. for 2 hours to obtain a zeolite-based catalyst.
[0054] Example 1
[0055] A method for preparing high-purity hydroxyethyl acrylate comprises the following steps:
[0056] S1, add 200kg acrylic acid and 1.5kg zeolite-based catalyst prepared in Preparation Example 2 into a condensation reactor, stir at a speed of 100rpm and heat with steam to 75°C, slowly introduce 130kg ethylene oxide into the reactor through the liquid, control the reaction temperature at 85°C, and keep the reaction temperature for 30min to obtain a crude product;
[0057] S2, adding the crude product to a distillation kettle, adding 0.09 kg of polymerization inhibitor 2,2,6,6-tetramethylpiperidinoxide, distilling under reduced pressure at 0.1 MPa, heating with steam to 100 ° C, and in continuous production, the distillation is terminated when the liquid level of the reaction liquid in the intermediate kettle is lower than the liquid level gauge, collecting the product, and obtaining a hydroxyethyl acrylate finished product and a distillation residue;
[0058] S3. The distillation residue enters the thin film evaporator again, and is heated to 92°C with steam. The product is collected to obtain hydroxyethyl acrylate finished product and distillation residue, and the distillation residue is concentrated for solid waste treatment.
[0059] Example 2
[0060] A method for preparing high-purity hydroxyethyl acrylate comprises the following steps:
[0061] S1, add 200kg acrylic acid and 1.7kg zeolite-based catalyst prepared in Preparation Example 3 into a condensation reactor, stir at a speed of 100rpm and heat with steam to 75°C, slowly introduce 132kg ethylene oxide into the reactor through the liquid, control the reaction temperature at 90°C, and keep the reaction temperature for 40min to obtain a crude product;
[0062] S2, adding the crude product to a distillation kettle, adding 0.092 kg of polymerization inhibitor 2,2,6,6-tetramethylpiperidinoxide, distilling under reduced pressure at 0.2 MPa, heating with steam to 105 ° C, and in continuous production, the distillation is terminated when the liquid level of the reaction liquid in the intermediate kettle is lower than the liquid level gauge, collecting the product, and obtaining a hydroxyethyl acrylate finished product and a distillation residue;
[0063] S3. The distillation residue enters the thin film evaporator again, and is heated to 96°C with steam. The product is collected to obtain hydroxyethyl acrylate finished product and distillation residue, and the distillation residue is concentrated for solid waste treatment.
[0064] Example 3
[0065] A method for preparing high-purity hydroxyethyl acrylate comprises the following steps:
[0066] S1, add 200kg acrylic acid and 1.8kg zeolite-based catalyst prepared in Preparation Example 4 into a condensation reactor, stir at a speed of 150rpm and heat with steam to 78°C, slowly introduce 136kg ethylene oxide into the reactor through the liquid, control the reaction temperature at 92°C, and keep the reaction temperature for 45min to obtain a crude product;
[0067] S2, adding the crude product to a distillation kettle, adding 0.095 kg of a polymerization inhibitor 2,2,6,6-tetramethylpiperidinoxide, distilling under reduced pressure at 0.3 MPa, heating with steam to 108° C., and in continuous production, the distillation is terminated when the liquid level of the reaction liquid in the intermediate kettle is lower than the liquid level gauge, collecting the product, and obtaining a hydroxyethyl acrylate finished product and a distillation residue;
[0068] S3. The distillation residue enters the thin film evaporator again, and is heated to 97°C with steam. The product is collected to obtain hydroxyethyl acrylate finished product and distillation residue, and the distillation residue is concentrated for solid waste treatment.
[0069] Example 4
[0070] A method for preparing high-purity hydroxyethyl acrylate comprises the following steps:
[0071] S1, add 200kg of acrylic acid and 2kg of the zeolite-based catalyst prepared in Preparation Example 2 into a condensation reactor, stir at a speed of 200rpm and heat with steam to 80°C, slowly introduce 140kg of ethylene oxide into the reactor through the liquid, control the reaction temperature at 95°C, and keep the reaction temperature for 60min to obtain a crude product;
[0072] S2, adding the crude product to a distillation kettle, adding 0.1 kg of polymerization inhibitor 2,2,6,6-tetramethylpiperidinoxide, distilling under reduced pressure at 0.5 MPa, heating with steam to 110° C., and in continuous production, the distillation is terminated when the liquid level of the reaction liquid in the intermediate kettle is lower than the liquid level gauge, collecting the product, and obtaining a hydroxyethyl acrylate finished product and a distillation residue;
[0073] S3. The distillation residue enters the thin film evaporator again, and is heated to 100°C with steam. The product is collected to obtain hydroxyethyl acrylate finished product and distillation residue. The distillation residue is concentrated for solid waste treatment.
[0074] Comparative Example 1
[0075] The difference between this comparative example and Example 1 is that the zeolite molecular sieve particles prepared in Preparation Example 2 are used instead of the zeolite-based catalyst, and the remaining steps are the same as those in Example 1.
[0076] Comparative Example 2
[0077] The difference between this comparative example and Example 2 is that the sodium vanadate solution prepared in Preparation Example 3 is used instead of the zeolite-based catalyst, and the remaining steps are the same as those in Example 2.
[0078] Comparative Example 3
[0079] The difference between this comparative example and Example 3 is that ferric chloride is used instead of the zeolite-based catalyst, and the remaining steps are the same as those of Example 3.
[0080] Comparative Example 4
[0081] The difference between this comparative example and Example 4 is that no catalyst is added, and the remaining steps are the same as those of Example 4.
[0082] The discharge conditions of Examples 1-4 and Comparative Examples 1-4 were recorded, and the results are shown in Table 1:
[0083] Table 1. Yield and purity of Examples 1-4 and Comparative Examples 1-4
[0084] serial number Hydroxyethyl acrylate(kg) Residue(kg) Impurities(kg) Example 1 329.34 2.08 0.17 Example 2 331.04 2.13 0.62 Example 3 334.78 2.35 0.77 Example 4 339.69 2.01 0.40 Comparative Example 1 302.14 28.03 1.42 Comparative Example 2 230.24 37.18 66.37 Comparative Example 3 321.77 12.28 3.85 Comparative Example 4 211.39 43.85 86.86
[0085] The hydroxyethyl acrylate samples prepared in Examples 1-4 and Comparative Examples 1-4 were tested for technical indicators (the test method refers to the enterprise standard Q / SH 001-2019 "Hydroxyethyl Acrylate"):
[0086] (I) Purity: Purity = (mass of hydroxyethyl acrylate / (mass of hydroxyethyl acrylate + mass of impurities)) x 100%.
[0087] (II) Chroma: measured in accordance with GB / T 3143-1982 “Method for determination of color of liquid chemical products (Hazen unit – platinum-cobalt color number)”.
[0088] (III) Free acid: Add about 50 mL of ethanol to a 150 mL conical flask, add a few drops of phenolphthalein solution as an indicator, slowly titrate with 0.1 mol / L NaOH solution until the solution color changes to slightly red and does not fade for 15 seconds, and immediately add 10 mL of the samples of Examples 1-4 and Comparative Examples 1-4 to the neutralized ethanol. Titrate with 0.1 mol / L standard sodium hydroxide solution. When the solution color changes from colorless to slightly red and does not fade within 15 seconds, it is considered as the titration end point. Record the volume (V1) of the sodium hydroxide solution consumed during the titration. Free acid (%) = (V1×c×M) / (V×G×10), where c is the molar concentration of the sodium hydroxide solution, M is the molecular weight of the free acid (in terms of acrylic acid), V is the sample amount (mL), G is the sample specific gravity at the measurement temperature, and V1 is the volume (mL) of the NaOH solution consumed.
[0089] (IV) Water content: Determined in accordance with GB / T 6283-2008 “Determination of water content in chemical products - Karl Fischer method (general method)”.
[0090] The results are shown in Table 2:
[0091] Table 2. Technical indicators of Examples 1-4 and Comparative Examples 1-4
[0092] serial number purity(%) Chroma Free acid (%) Moisture (%) Example 1 99.95 14 0.10 0.08 Example 2 99.82 13 0.14 0.09 Example 3 99.78 18 0.14 0.08 Example 4 99.89 16 0.11 0.07 Comparative Example 1 99.47 29 0.65 0.10 Comparative Example 2 77.78 56 2.02 0.05 Comparative Example 3 98.73 16 0.82 0.08 Comparative Example 4 70.77 68 2.13 0.09
[0093] As can be seen from Table 1 and Table 2, the yield and purity of Examples 1-4 are both high, indicating that the zeolite-based catalyst has high catalytic activity and selectivity in this reaction, and can effectively promote the condensation reaction of acrylic acid and ethylene oxide while reducing the generation of by-products. Comparative Example 1 uses zeolite molecular sieve particles without sodium vanadate as a catalyst, and its yield and purity are lower than those of Example 1. Comparative Example 2 uses sodium vanadate solution as a catalyst, which may be due to its poor dispersibility or insufficient active sites, resulting in low yield and purity. Comparative Example 3 uses ferric chloride as a catalyst, and its yield is close to that of the embodiment, but the purity is low, indicating that although ferric chloride has certain catalytic activity, it is not as good as zeolite-based catalysts in terms of selectivity.
[0094] Specifically, in Table 2, the chromaticity of Examples 1-4 is at a relatively low level (13-18 Hazen units), indicating that the product color is lighter. The chromaticity of Comparative Example 1 is 29 Hazen units, which is higher than that of the embodiment. The chromaticity of Comparative Example 2 and Comparative Example 4 is extremely high, 56 and 68 Hazen units, respectively, indicating that the product color is darker, which may be caused by more by-products. The chromaticity of Comparative Example 3 is 16 Hazen units, which is similar to that of the embodiment, indicating that the ferric chloride catalyst has little effect on the product color.
[0095] The free acid content of Examples 1-4 is at a relatively low level (0.10-0.14%), indicating that the content of free acid (acrylic acid) in the product is very small. The free acid content of Comparative Example 1 is 0.65%, which is higher than that of the Example. The free acid content of Comparative Example 2 and Comparative Example 4 is relatively high, 2.02% and 2.13% respectively, which may be due to the incomplete reaction caused by the poor catalyst effect, and more free acid remains in the product. The free acid content of Comparative Example 3 is 0.82%, which is higher than that of the Example but lower than that of Comparative Example 2 and Comparative Example 4, indicating that the ferric chloride catalyst has a certain effect in reducing free acid, but is not as good as the zeolite-based catalyst.
[0096] The difference in moisture content between Examples 1-4 and Comparative Examples 1-4 is not significant, indicating that the zeolite-based catalyst has little effect on the moisture content in the product.
[0097] In summary, the preparation methods of Examples 1-4 can prepare high-purity hydroxyethyl acrylate with high yield and low impurity content. The zeolite-based catalyst exhibits high catalytic activity and selectivity in this reaction, which is superior to other comparative catalysts.
[0098] In the description of the specification, the description with reference to the terms "preparation example", "embodiment", "various embodiments" and the like means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or preparation example are included in at least one embodiment or preparation example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or preparation example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or preparation examples in a suitable manner.
[0099] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing high-purity hydroxyethyl acrylate, It is characterized in that The following steps are involved: S1, adding acrylic acid and zeolite-based catalyst into a condensation reaction kettle, stirring and heating with steam, passing ethylene oxide into the reaction kettle through liquid, controlling the reaction temperature, and keeping the temperature to react to obtain a crude product; S2, adding the crude product to a distillation kettle, adding a polymerization inhibitor, performing vacuum distillation, heating with steam to raise the temperature, collecting the product, and obtaining a hydroxyethyl acrylate finished product and a distillation residue; S3. The distillation residue enters the thin film evaporator again, is heated by steam, and the product is collected to obtain the hydroxyethyl acrylate finished product and distillation residue, which is then concentrated for solid waste treatment.
2. A method for preparing high-purity hydroxyethyl acrylate according to claim 1, It is characterized in that In step S1, the steam heating temperature is 75-80°C, the stirring speed is 100-200rpm, and after the ethylene oxide is introduced, the reaction temperature is controlled at 85-95°C, and the insulation time is 30-60min.
3. A method for preparing high-purity hydroxyethyl acrylate according to claim 1, It is characterized in that The pressure of the reduced pressure distillation in step S2 is 0.1-0.5 MPa, and the temperature of the steam heating is 100-110°C.
4. A method for preparing high-purity hydroxyethyl acrylate according to claim 1, It is characterized in that The temperature of steam heating in step S3 is 92-100°C.
5. A method for preparing high-purity hydroxyethyl acrylate according to claim 1, It is characterized in that The feed mass ratio of acrylic acid, ethylene oxide, zeolite-based catalyst and polymerization inhibitor is 2000:(1300-1400):(15-20):(0.9-1), and the polymerization inhibitor is 2,2,6,6-tetramethylpiperidinoxide.
6. A method for preparing high-purity hydroxyethyl acrylate according to claim 1, It is characterized in that The zeolite-based catalyst in step S1 is prepared by the following steps: A1. Add tetrapropylammonium hydroxide to deionized water, adjust the pH value to 10-11 with sodium hydroxide, add silica sol and aluminum sol under continuous stirring, transfer to an autoclave with a polytetrafluoroethylene liner, seal, place in an oven for crystallization, cool to room temperature, filter, wash, and dry to obtain zeolite molecular sieve particles; A2. Add vanadate powder into deionized water and heat to 80-90° C. to prepare a 0.1-0.5 mol / L vanadate solution; A3. Add zeolite molecular sieve particles into vanadate solution and immerse for 2-3 hours, filter, wash, and then place in a muffle furnace for solidification to obtain a zeolite-based catalyst.
7. A method for preparing high-purity hydroxyethyl acrylate according to claim 6, It is characterized in that In step A1, the mass ratio of tetrapropylammonium hydroxide, deionized water, silica sol and aluminum sol is (5-7):50:(25-30):(1-1.5).
8. A method for preparing high-purity hydroxyethyl acrylate according to claim 6, It is characterized in that In step A1, the crystallization temperature is 170-180° C., and the crystallization time is 48-72 h.
9. A method for preparing high-purity hydroxyethyl acrylate according to claim 6, It is characterized in that The vanadate in step A2 includes one of sodium vanadate, potassium vanadate, bismuth vanadate, strontium vanadate, sodium ammonium vanadate, calcium vanadate, magnesium vanadate, and indium vanadate.
10. A method for preparing high-purity hydroxyethyl acrylate according to claim 6, It is characterized in that In step A3, the mass ratio of zeolite molecular sieve particles to vanadate solution is (8-15): (20-26), the curing temperature is 600-700° C., and the curing time is 1-2 h.