Preparation method of transparent ceramic for direct detection of visible light and X rays

Through the control of temperature and pressure through hot pressing engineering, the problem of insufficient density of perovskite ceramics is solved, its transparency and charge transport performance are improved, and the performance performance of visible light and X-ray detectors is improved.

CN118930437APending Publication Date: 2024-11-12SUZHOU YIXIAN ELECTRONIC TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996840.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The application of perovskite in the field of X-ray detectors is limited by problems such as insufficient density, high defect density and obvious grain boundaries, resulting in low transparency and low charge carrier collection efficiency, which affects the detector performance and working stability.

Method used

Fine hot pressing engineering is adopted to regulate temperature, pressure and time, and high transparency perovskite ceramics with controllable thickness are prepared to improve charge transfer performance and reduce dark current.

Benefits of technology

It improves the density and crystallinity of perovskite ceramics, enhances its application capabilities in visible light and X-ray detectors, and improves the efficiency and stability of the detector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930437A_ABST
    Figure CN118930437A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of transparent ceramic for direct detection of visible light and X rays, which comprises the following steps: dissolving BX2 and AX in an organic solvent to obtain an ABX3 perovskite precursor solution; heating, stirring and separating out the ABX3 perovskite precursor solution to obtain ABX3 microcrystals; and grinding the ABX3 microcrystals, and carrying out fine hot pressing engineering treatment to obtain the APbX3 transparent ceramic. By finely regulating and controlling the hot pressing pressure, temperature and time, on one hand, re-growth of the perovskite wafer with relatively high defect density is promoted, the crystallinity of the wafer is improved, the defect density is reduced, the air stability is improved, and the perovskite wafer has good optical transparency; and on the other hand, under the combined action of hot pressing pressure, temperature and time, device surface grain boundary fusion is further promoted, the charge transmission performance is improved, and dark current is reduced, so that high-efficiency visible light and X-ray direct detection is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of visible light detection and X-ray detection, and in particular to a method for preparing transparent ceramics used in visible light detection and X-ray imaging. Background Art

[0002] In medical imaging, the combination of visible light and X-ray imaging can provide more comprehensive and accurate diagnostic information. Visible light images can show the surface of the skin, while X-ray images can look deep into the body to observe bone or tissue structures. By combining these two imaging technologies, doctors can obtain more dimensional information, which helps to diagnose diseases more accurately. In the industrial field, the combination of visible light detection and X-ray imaging can also improve the efficiency and accuracy of material detection. Visible light images can show defects or foreign objects on the external surface, while X-ray images can detect whether the internal structure is intact. By comprehensively analyzing these two types of imaging data, the quality and performance of materials can be more comprehensively evaluated. In general, the combination of visible light detection and X-ray imaging can bring us more comprehensive and accurate information in many fields, which helps to improve work efficiency and accuracy.

[0003] Perovskite has great application potential in the field of visible light and direct X-ray detection due to its advantages such as high photon absorption efficiency, large carrier mobility and long carrier lifetime. In order to fully absorb visible light and reduce the scattering of visible light, the perovskite active layer should have high transparency. In addition, in order to fully absorb high-energy X-rays, the thickness of the perovskite active layer should reach hundreds of microns. At present, the application of perovskite in X-ray is mainly based on single crystal and thin film, but the growth of perovskite single crystal is time-consuming and difficult to prepare on a large scale. Due to the limited solubility of the precursor, it is also difficult to prepare a perovskite thick film that meets the requirements by solution method. Compacting perovskite powder to form a polycrystalline perovskite wafer can construct a perovskite X-ray detection photosensitive layer with adjustable size and thickness, but the polycrystalline inorganic perovskite wafer prepared in this way usually contains many voids and grain boundaries. The prepared polycrystalline wafer has problems such as low transparency and insufficient density, which increases the scattering of visible light, affects the effective collection of charge carriers, and ultimately restricts the performance of the detector. In addition, it seriously affects the efficiency and working stability of the X-ray detector, and it is difficult to further integrate it with the substrate circuit.

[0004] In summary, in order to further promote the application of perovskite materials in the field of visible light and X-ray detectors, it is necessary to improve the quality of perovskite crystals and perovskite thick films to prepare high-performance visible light / X-ray detectors. Summary of the invention

[0005] In order to solve the above-mentioned problems existing in the prior art, the present invention proposes a method for preparing transparent ceramics for direct detection of visible light and X-rays. Through precise hot pressing engineering, the interaction between factors such as temperature, pressure, and time is fully regulated to solve the problems of insufficient density, high defect density, and obvious grain boundaries of perovskite ceramics, and prepare perovskite ceramics with controllable thickness and high transparency; thereby improving the charge transfer performance and reducing the dark current, thereby obtaining efficient visible light detection and X-ray imaging application capabilities.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing transparent ceramics for direct detection of visible light and X-rays comprises the following steps:

[0008] Step 1: preparing ABX3 microcrystalline powder: dissolving BX2 and AX in an organic solvent to obtain an ABX3 perovskite precursor solution, precipitating by heating and stirring to obtain ABX3 microcrystalline, drying, and grinding to obtain ABX3 microcrystalline powder with uniform particles;

[0009] The ABX3, wherein A is a methylamine cation CH3NH3 + 、Formamidinium cation HC(NH2)2 + or Cesium ion Cs + One or more mixed cations in; B is a metal ion, a germanium ion Ge 2+ 、Sn 2+ or lead ion Pb 2+ One or more mixed metal ions; X halogen ion is iodine I - , Br - or chlorine - One or more mixed halogen elements;

[0010] The molar ratio of BX2 to AX is 1:1-2; the organic solvent is N,N-dimethylformamide DMF and dimethyl sulfoxide;

[0011] Step 2: Prepare the wafer: Place the ABX3 microcrystalline powder into the hot pressing mold; set the corresponding temperature, pressure and time parameters, and start the pressurization process after the heating temperature reaches the set value; after the hot pressing is completed, open the mold after the equipment cools down and take out the transparent ceramic prepared by hot pressing.

[0012] Preferably, in the process of preparing ABX3 microcrystalline powder, the dissolution is stirring dissolution, the heating and stirring rate is 200-1000 rpm; the heating and stirring time is 1-6 hours, and the heating temperature is 60-120°C.

[0013] Preferably, the heating and stirring rate is 800 rpm; and the heating and stirring time is 3 h.

[0014] Preferably, in the process of preparing ABX3 microcrystalline powder, the concentration of ABX3 perovskite precursor solution is 0.6-1.5 mol / L.

[0015] Preferably, the concentration of the ABX3 perovskite precursor solution is 1 mol / mL.

[0016] Preferably, in the process of preparing ABX3 microcrystalline powder, the drying is vacuum drying at a temperature of 40 to 60° C. for a drying time of 24 to 36 hours, after which dried perovskite ABX3 microcrystals are obtained.

[0017] Preferably, in the process of preparing the ABX3 microcrystalline powder, the grinding is performed using an agate mortar, and the grinding is repeated 3 to 5 times, with each grinding time being 30 to 60 minutes, until a perovskite powder with a particle size of about 50 μm is obtained.

[0018] Preferably, in the process of preparing the wafer, the hot pressing mold is a tungsten steel mold with a diameter of 3mm-100mm.

[0019] Preferably, the prepared wafer is pressed under high temperature and high pressure, the high pressure is 10-400 MPa, the high temperature is 80-150° C., and the pressure holding time of the pressed wafer is 10-120 min.

[0020] Preferably, the hot pressing mold has a diameter of 10 mm, the high pressure is 200 MPa, and is cooled to 50°C.

[0021] Preferably, during the wafer preparation process, the equipment is cooled by natural cooling to 25-50°C.

[0022] The transparent ceramic prepared by the method of the present invention is used to prepare a high-performance visible light / X-ray detector, which can respectively detect the visible light signal and the X-ray signal of an object, thereby improving the object recognition capability.

[0023] Beneficial effects:

[0024] (1) Compared with the original method, the method for preparing transparent ceramics provided by the present invention can prepare ceramics with good optical transparency.

[0025] (2) The method for preparing transparent ceramics provided by the present invention promotes the regrowth of perovskite wafers with high defect density, improves the crystallinity of the wafers, reduces the defect density, and improves air stability.

[0026] (3) The preparation method of transparent ceramics provided by the present invention, under the combined effects of hot pressing pressure, temperature and time, further promotes the fusion of grain boundaries on the device surface, improves the charge transfer performance, and reduces the dark current, thereby obtaining efficient visible light detection and X-ray imaging application capabilities.

[0027] (4) This method is simple to operate, novel and unique, and can obtain transparent ceramics with controllable thickness and area and high crystal quality without the use of large amounts of solvents and complex and expensive equipment, and has the potential for large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the transparent ceramic preparation method of the present invention;

[0029] Figure 2-5 Optical images of transparent ceramics prepared in Comparative Examples 1-4 of the present invention;

[0030] Figure 6 This is an optical picture of the transparent ceramic prepared in Example 1 of the present invention;

[0031] Figure 7 This is the XRD spectrum of the MAPbBr3 transparent ceramic in Example 1 of the present invention. DETAILED DESCRIPTION

[0032] The present invention will be further described below in conjunction with specific embodiments and accompanying drawings:

[0033] Comparative Example 1

[0034] Experimental steps for preparing MAPbBr3 metal halide perovskite transparent ceramics (such as Figure 1 shown):

[0035] (1) Lead bromide and methylamine bromide are dissolved in N,N-dimethylformamide and stirred in a beaker until completely dissolved at a stirring rate of 800 rpm. The solution is filtered using a 22 μm organic filter to form a clear and transparent MAPbBr3 precursor solution, wherein the molar ratio of lead bromide to methylamine bromide is 1:1. 2+ The concentration is 1M;

[0036] (2) The solution prepared in step 2 was placed on a stirring heater, the temperature was set to 80°C, the stirring rate was 800 rpm and the heating and stirring were continued for 3 hours. As the solubility of the solution decreased, MAPbBr3 microcrystals gradually precipitated. The precipitated microcrystals were placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0037] (3) Grind the dried MAPbBr3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 minutes, until a MAPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0038] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 50°C and 10 MPa for 10 minutes to press the chip. In this embodiment, the thickness of the ceramic obtained by pressing is about 600 μm.

[0039] (5) After the hot pressing is completed, wait for the equipment to cool to 50°C before opening the mold and taking out the hot pressed wafer. The actual picture is as follows Figure 2 shown.

[0040] Comparative Example 2

[0041] This comparative example is basically the same as comparative example 1, except that the hot pressing pressure is 100 MPa.

[0042] Experimental steps for preparing MAPbBr3 metal halide perovskite transparent ceramics (such as Figure 1 shown):

[0043] (1) Lead bromide and methylamine bromide are dissolved in N,N-dimethylformamide and stirred in a beaker until completely dissolved at a stirring rate of 800 rpm. The solution is filtered using a 22 μm organic filter to form a clear and transparent MAPbBr3 precursor solution, wherein the molar ratio of lead bromide to methylamine bromide is 1:1. 2+ The concentration is 1M;

[0044] (2) The solution prepared in step 2 was placed on a stirring heater, the temperature was set to 80°C, the stirring rate was 800 rpm and the heating and stirring were continued for 3 hours. As the solubility of the solution decreased, MAPbBr3 microcrystals gradually precipitated. The precipitated microcrystals were placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0045] (3) Grind the dried MAPbBr3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 minutes, until a MAPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0046] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 50°C and 100 MPa for 10 minutes to press the chip. In this embodiment, the thickness of the ceramic obtained by pressing is about 600 μm.

[0047] (5) After the hot pressing is completed, wait for the equipment to cool to 50°C before opening the mold and taking out the hot pressed wafer. The actual picture is as follows Figure 3 shown.

[0048] Comparative Example 3

[0049] This comparative example is basically the same as comparative example 1, except that the hot pressing pressure is 200 MPa.

[0050] Experimental steps for preparing MAPbBr3 metal halide perovskite transparent ceramics (such as Figure 1 shown):

[0051] (1) Lead bromide and methylamine bromide are dissolved in N,N-dimethylformamide and stirred in a beaker until completely dissolved at a stirring rate of 800 rpm. The solution is filtered using a 22 μm organic filter to form a clear and transparent MAPbBr3 precursor solution, wherein the molar ratio of lead bromide to methylamine bromide is 1:1. 2+ The concentration is 1M;

[0052] (2) The solution prepared in step 2 was placed on a stirring heater, the temperature was set to 80°C, the stirring rate was 800 rpm and the heating and stirring were continued for 3 hours. As the solubility of the solution decreased, MAPbBr3 microcrystals gradually precipitated. The precipitated microcrystals were placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0053] (3) Grind the dried MAPbBr3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 minutes, until a MAPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0054] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 50°C and 200 MPa for 10 minutes to press the chip. In this embodiment, the thickness of the ceramic obtained by pressing is about 600 μm.

[0055] (5) After the hot pressing is completed, wait for the equipment to cool to 50°C before opening the mold and taking out the hot pressed wafer. The actual picture is as follows Figure 4 shown.

[0056] Comparative Example 4

[0057] This comparative example is basically the same as comparative example 1, the only difference being that the holding time is 30 min and the hot pressing pressure is 200 MPa.

[0058] Experimental steps for preparing MAPbBr3 metal halide perovskite transparent ceramics (such as Figure 1 shown):

[0059] (1) Dissolve lead bromide and methylamine bromide in N,N-dimethylformamide, and stir in a beaker until completely dissolved at a stirring rate of 800 rpm. Filter the solution using a 22 μm organic filter to form a clear and transparent MAPbBr3 precursor solution, wherein the molar ratio of lead bromide to methylamine bromide is 1:1. The Pb2+ concentration is 1 M;

[0060] (2) The solution prepared in step 2 was placed on a stirring heater, the temperature was set to 80°C, the stirring rate was 800 rpm and the heating and stirring were continued for 3 hours. As the solubility of the solution decreased, MAPbBr3 microcrystals gradually precipitated. The precipitated microcrystals were placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0061] (3) Grind the dried MAPbBr3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 minutes, until a MAPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0062] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 50°C and 200 MPa for 30 minutes to press the chip. In this embodiment, the thickness of the ceramic obtained by pressing is about 600 μm.

[0063] (5) After the hot pressing is completed, wait for the equipment to cool to 50°C before opening the mold and taking out the hot pressed wafer. The actual picture is as follows Figure 5 shown.

[0064] from Figure 3 It can be seen that the thickness change of the wafer is successfully regulated by changing the thickness of the substrate spacing layer of the present invention.

[0065] from Figure 4 It can be seen that the single crystal thick film obtained by the single crystal thick film growth apparatus of the present invention has a regular shape and a large area.

[0066] from Figure 5 It is found that the wafer obtained by the growth method of the present invention has good crystallinity.

[0067] For the optical images of the prepared ceramics in Comparative Examples 1-4 above, factors such as temperature, pressure, time, etc. during the hot pressing process affect the optical and electrical properties of the perovskite wafer. The interaction between various factors is considered to improve the transparency, density, and effective collection of charge carriers, and ultimately improve the performance of the detector.

[0068] Example 1

[0069] Experimental steps for preparing MAPbBr3 metal halide perovskite transparent ceramics (such as Figure 1 shown):

[0070] (1) Lead bromide and methylamine bromide are dissolved in N,N-dimethylformamide and stirred in a beaker until completely dissolved at a stirring rate of 800 rpm. The solution is filtered using a 22 μm organic filter to form a clear and transparent MAPbBr3 precursor solution, wherein the molar ratio of lead bromide to methylamine bromide is 1:1. 2+ The concentration is 1M;

[0071] (2) The solution prepared in step 2 was placed on a stirring heater, the temperature was set to 80°C, the stirring rate was 800 rpm and the heating and stirring were continued for 3 hours. As the solubility of the solution decreased, MAPbBr3 microcrystals gradually precipitated. The precipitated microcrystals were placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0072] (3) Grind the dried MAPbBr3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 minutes, until a MAPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0073] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 50°C and 10 MPa for 10 minutes to press the chip. In this embodiment, the thickness of the ceramic obtained by pressing is about 600 μm.

[0074] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 150°C and 200 MPa for 60 minutes to press the chip. In this embodiment, the thickness of the transparent ceramic obtained by pressing is about 600 μm.

[0075] (5) After the hot pressing is completed, wait for the equipment to cool to 50°C before opening the mold and taking out the hot pressed wafer. The actual picture is as follows Figure 6 The perovskite ceramics prepared by the preparation method of the present invention have good optical transparency, and the XRD spectrum (such as Figure 7 (as shown) indicates that the prepared MAPbBr3 transparent ceramics have good crystallinity.

[0076] Example 2

[0077] Experimental steps for preparing MAPbCl3 metal halide perovskite transparent ceramics:

[0078] (1) Lead bromide and methylamine bromide are dissolved in a mixed solution of N,N-dimethylformamide and dimethyl sulfoxide (VDMF:VDMSO=1:1), and stirred in a beaker until completely dissolved at a stirring rate of 800 rpm. The solution is filtered using a 22 μm organic filter to form a clear and transparent MAPbCl3 precursor solution, wherein the molar ratio of lead chloride to methylamine chloride is 1:1. 2+ The concentration is 1M;

[0079] (2) The solution prepared in step 2 was placed on a stirring heater, the temperature was set to 60°C, the stirring rate was 800 rpm and the heating and stirring were continued for 3 hours. As the solubility of the solution decreased, MAPbCl3 microcrystals gradually precipitated. The precipitated microcrystals were placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0080] (3) Grind the dried MAPbCl3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 min, until a MAPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0081] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 150°C and 200 MPa for 60 minutes to press the chip. In this embodiment, the thickness of the transparent ceramic obtained by pressing is about 600 μm.

[0082] (5) After the hot pressing is completed, wait for the equipment to cool to 50° C. before opening the mold and taking out the transparent ceramic prepared by hot pressing.

[0083] Example 3

[0084] Experimental steps for preparing CsPbBr3 metal halide perovskite transparent ceramics

[0085] (1) Lead bromide and cesium bromide are dissolved in dimethyl sulfoxide, stirred in a beaker and a small amount of hydrobromic acid is added dropwise to dissolve, and the stirring rate is 800 rpm. The solution is filtered using a 22 μm organic filter to form a clear and transparent CsPbBr3 precursor solution, wherein the molar ratio of lead bromide to cesium bromide is 2:1, and the molar ratio of Pb to Cs is 1:1. 2+ The concentration is 1.6M;

[0086] (2) The solution prepared in step 2 is placed on a stirring heater, the temperature is set to 110°C, the stirring rate is 800 rpm and the heating and stirring are continued for 3 hours. As the solubility of the solution decreases, CsPbBr3 microcrystals gradually precipitate. The precipitated microcrystals are placed in a vacuum dryer at 60°C and dried for 12 hours and then taken out.

[0087] (3) Grind the dried CsPbBr3 microcrystals in an agate mortar and repeat the grinding for 3 to 5 times, with each grinding time being 30 to 60 minutes, until a CsPbBr3 perovskite microcrystal powder with a particle size of about 50 μm is obtained.

[0088] (4) Weigh an appropriate amount of perovskite powder and put it into a hot pressing mold. Select a mold with a size of 10 cm*10 cm and use a hydraulic press to press it at 150°C and 200 MPa for 60 minutes to press the chip. In this embodiment, the thickness of the transparent ceramic obtained by pressing is about 600 μm.

[0089] (5) After the hot pressing is completed, wait for the equipment to cool to 50° C. before opening the mold and taking out the transparent ceramic prepared by hot pressing.

[0090] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a transparent ceramic for direct detection of visible light and X-rays, characterized in that: The following steps are involved: Step 1: preparing ABX3 microcrystalline powder: dissolving BX2 and AX in an organic solvent to obtain an ABX3 perovskite precursor solution, precipitating by heating and stirring to obtain ABX3 microcrystalline, drying, and grinding to obtain ABX3 microcrystalline powder with uniform particles; The ABX3, wherein A is a methylamine cation CH3NH3 + 、Formamidinium cation HC(NH2)2 + or Cesium ion Cs + One or more mixed cations in; B is a metal ion, a germanium ion Ge 2+ 、Sn 2+ or lead ion Pb 2+ One or more mixed metal ions; X halogen ion is iodine I - , Br - or chlorine - One or more mixed halogen elements; The molar ratio of BX2 to AX is 1:1-2; the organic solvent is N,N-dimethylformamide DMF and dimethyl sulfoxide; Step 2: Prepare the wafer: Place the ABX3 microcrystalline powder into the hot pressing mold; set the temperature, pressure and time parameters, and start the pressurization process after the heating temperature reaches the set value; after the hot pressing is completed, open the mold after the equipment cools down and take out the transparent ceramic prepared by hot pressing.

2. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 1, characterized in that: In the process of preparing ABX3 microcrystalline powder, the dissolution is stirring dissolution, the heating and stirring rate is 200-1000 rpm; the heating and stirring time is 1-6 hours, and the heating temperature is 60-120°C.

3. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 2, characterized in that: The heating and stirring rate is 800 rpm; the heating and stirring time is 3 h.

4. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 3, characterized in that: In the process of preparing the ABX3 microcrystalline powder, the concentration of the ABX3 perovskite precursor solution is 0.6-1.5 mol / L.

5. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 4, characterized in that: The concentration of the ABX3 perovskite precursor solution is 1 mol / mL.

6. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 5, characterized in that: In the process of preparing the ABX3 microcrystalline powder, the drying is vacuum drying at a temperature of 40 to 60° C. and a drying time of 24 to 36 hours, after which dry perovskite ABX3 microcrystals are obtained; the grinding is grinding in an agate mortar, and the grinding is repeated 3 to 5 times, each grinding time being 30 to 60 minutes, until a perovskite powder with a particle size of about 50 μm is obtained.

7. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 6, characterized in that: In the process of preparing the wafer, the hot pressing mold is a tungsten steel mold with a diameter of 3mm-100mm.

8. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 7, characterized in that: The prepared wafer is pressed under high temperature and high pressure, the high pressure is 10-400MPa, the high temperature is 80-150°C, and the pressure holding time of the pressed wafer is 10-120min.

9. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 8, characterized in that: The hot pressing mold has a diameter of 10 mm, the high pressure is 200 MPa, and is cooled to 50°C.

10. The method for preparing a transparent ceramic for direct detection of visible light and X-rays according to claim 9, characterized in that: During the wafer preparation process, the equipment is cooled by natural cooling to 25-50°C.