Preparation method and application of higher fatty acid monoester polyol taking illegal cooking oil as raw material
Preparation of high-grade fatty acid monoester polyols through gutter oil solves the problems of flammable and low flame retardant properties of bio-based polyurethanes, achieving high-efficiency and green flame retardant effects and excellent mechanical properties, avoiding the harm and phase of traditional flame retardants Capacity issues.
Patent Information
- Application Number
- CN202410999223.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing bio-based polyurethane materials are flammable and have low flame retardant properties, and the traditional flame retardant is added large and the compatibility is poor, which affects the mechanical properties and poses safety hazards.
Using gutter oil as raw material to prepare high-grade fatty acid monoester polyols, by dropping high-grade fatty acid monoester and epoxy compound into the phosphoric acid-containing compound, a bio-based polyurethane flame retardant with excellent mechanical properties was prepared. Water phosphoric acid or pyrophosphate catalyzed the reaction, controlling the reaction conditions to avoid violent reactions.
It achieves green and environmentally friendly, efficient flame retardant and excellent mechanical properties, avoids the gas release and compatibility problems of traditional flame retardants, reduces costs, and improves the flame retardant effect and material stability of polyurethane.
Smart Images

Figure CN118930578A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyurethane materials, and in particular to a preparation method of higher fatty acid monoester polyol using waste oil as a raw material and application thereof. Background Art
[0002] As the global use of petroleum energy increases, non-renewable resources such as oil are becoming increasingly depleted, and the prices of petroleum and petrochemical products continue to rise, people are paying attention to reducing the dependence on and use of petroleum-based plastic products. In order to fundamentally solve this problem, researchers are exploring the use of green, sustainable and renewable resources to replace petrochemical raw materials. With the increasing depletion of petroleum resources and increasingly stringent environmental legislation, there is an urgent need to develop environmentally friendly waterborne polyurethane (WPU) coatings.
[0003] With the increasing depletion of non-renewable fossil resources, the country's increased efforts to control environmental pollution and people's higher requirements for flame retardant properties of materials, the research on the use of renewable natural biomass resources to replace fossil resources to prepare environmentally friendly bio-based flame retardant polyurethane foam insulation materials has received widespread attention. The main raw materials of bio-based polyols, such as biodiesel, vegetable oil, fatty acids or dimerized fatty acids, have a wide range of sources, including castor oil, peanut oil, soybean oil, olive oil, neem oil, cottonseed oil, etc.
[0004] However, bio-based polyurethane is a flammable material. The limiting oxygen index (LOI) of ordinary polyurethane is very low, and the general LOI value is about 18%, which is very easy to cause combustion. At the same time, the combustion process is accompanied by the release of heat and smoke, and the dripping of molten droplets causes secondary combustion. In order to solve the above problems, flame retardants can generally be added to make bio-based polyurethane flame retardant. Specifically, flame retardants are added in the process of synthesizing polymers by physical incorporation. Halogen-containing, phosphorus-nitrogen-containing compounds, as well as traditional flame retardants such as aluminum hydroxide and magnesium hydroxide are usually added. However, these physical flame retardants are added in large amounts, are easy to precipitate, have poor compatibility with polyurethane, and affect the mechanical properties of the material. Halogen-containing flame retardants release a large amount of toxic gases during combustion, and have long been restricted in international use requirements. Therefore, it is urgent to develop a new, low-toxic, high-atomic-utilization and environmentally friendly new method. Summary of the invention
[0005] Purpose of the invention: In view of the problems existing in the existing flame retardants, the present invention provides a method for preparing a higher fatty acid monoester polyol using waste cooking oil as a raw material. The present invention can prepare a green, environmentally friendly, highly flame-retardant, and excellent mechanical property bio-based polyurethane flame retardant, and solves the problems that the existing bio-based polyurethane has low self-flammability, the addition of flame retardants affects the mechanical properties, and there are safety hazards during use, and provides a highly flame-retardant, excellent mechanical property, green and environmentally friendly bio-based polyurethane flame retardant.
[0006] The invention also provides the higher fatty acid monoester polyol and application thereof.
[0007] Technical solution: In order to achieve the above-mentioned purpose, the present invention discloses a method for preparing a higher fatty acid monoester polyol using waste cooking oil as raw material, comprising the following steps: dropping a higher fatty acid monoester into a phosphoric acid-containing compound for reaction, and then dropping an epoxy compound for reaction to obtain a higher fatty acid monoester polyol, wherein the phosphoric acid-containing compound is anhydrous phosphoric acid or pyrophosphoric acid.
[0008] Wherein, the anhydrous phosphoric acid is phosphoric acid with a purity greater than or equal to 98%.
[0009] The higher fatty acid monoester is derived from treated waste cooking oil, and the higher fatty acid monoester includes any one or more of epoxy methyl ester, palmitoleic acid methyl ester, linoleic acid methyl ester and stearic acid methyl ester.
[0010] Wherein, the epoxy compound is one or more of ethylene oxide, propylene oxide, epichlorohydrin, monohalogenated ethylene oxide, monohalogenated propylene oxide, dihalogenated ethylene oxide, and dihalogenated propylene oxide.
[0011] Wherein, the molar ratio of the phosphoric acid-containing compound, the higher fatty acid monoester and the epoxy compound is 1:0.5-3:1.5-8.
[0012] Preferably, the molar ratio of the phosphoric acid-containing compound, methyl epoxy ester and propylene oxide is 1.02:2.83:6.2.
[0013] The preparation method of the higher fatty acid monoester polyol of the present invention comprises the following steps:
[0014] Take anhydrous phosphoric acid or pyrophosphoric acid, put it in a reaction device, add higher fatty acid monoester and epoxy compound, and keep the temperature to react until the reaction is completed.
[0015] Among them, a higher fatty acid monoester is added dropwise at room temperature, and after the addition is completed, the mixture is kept warm at 50-100° C. for 1-5 hours; then, an epoxy compound is added dropwise at 50-100° C. in three batches, and after each batch is added, the mixture is kept warm for 1-5 hours.
[0016] Furthermore, after the epoxy compound is added dropwise and the reaction is completed, the epoxy compound is slowly and uniformly added dropwise after the temperature stabilizes. The dropping speed should be strictly controlled not to be too fast to prevent violent reaction and boiling. After the epoxy compound is added dropwise, the temperature is kept for 1 to 5 hours to allow full reaction. A constant pressure dropping funnel should be used for the epoxy compound addition and the dropping speed should be controlled to one drop per 5 to 10 seconds. Because the reaction is violent, too fast a dropping speed will cause boiling, and the epoxy compounds will react with each other.
[0017] Preferably, the preparation method comprises the following steps:
[0018] (1) Place 52.00 g of 85% phosphoric acid and 42.72 g of xylene in a single-mouth bottle equipped with a magnet, a water separator and a condenser, place it in an oil bath at 160°C, and start distillation for 12 hours. When the water level in the water separator no longer changes, stop distillation. Separate the phosphoric acid and xylene solution, take the lower layer of liquid, and obtain anhydrous phosphoric acid with a purity of 98-99%;
[0019] (2) Take the phosphoric acid after the reaction in step (1), put it in a four-necked flask equipped with a thermometer, a condenser, and a stirring rod, and add the higher fatty acid alkyl ester prepared from waste oil dropwise at room temperature. After the addition is completed, keep the temperature at 90° C. for 4 hours. Then, add propylene oxide dropwise at 90° C. in three batches, and keep the temperature for 2 hours after each batch is added.
[0020] The higher fatty acid monoester polyol is prepared by the method for preparing the higher fatty acid monoester polyol of the present invention.
[0021] The higher fatty acid monoester polyol is a colorless or light yellow viscous oligomeric phosphoric (phosphonic) ester phosphoric acid containing one or two or more -P(O)OH structures in the middle of the chain.
[0022] The invention discloses an application of the higher fatty acid monoester polyol as a flame retardant in the preparation of highly flame-retardant polyurethane foam plastics.
[0023] The higher fatty acid monoester bio-based flame retardant polyol prepared by the present invention using a specific method is a colorless or light yellow slightly viscous clear oily liquid with an acid value of ≤1 mgKOH / g. In the application of polyurethane foam, the acid will prevent the normal function of the amine catalyst used in the foaming reaction, and the foam will not rise, or the pore size is inappropriate, or the foam is sticky and fragile. The flame retardant of the present invention has a low acid value and does not affect the preparation of the foam and the basic properties of the material.
[0024] The present invention is a bio-based flame-retardant polyol that can be added to polyurethane. The raw materials are derived from renewable resources and are green and environmentally friendly. The green and environmentally friendly phosphorus element is introduced, which can be cracked to produce phosphoric acid molecules to play a flame retardant role when combustion occurs, and avoids the release of a large amount of toxic smoke during the combustion process; at the same time, the bio-based polyurethane is dehydrated and carbonized during combustion, and a coke layer is formed on the surface of the combustion object to isolate the combustion environment, which can further improve the flame retardant effect. Thereby, the overall flame retardant effect is achieved, and it has high-efficiency flame retardancy. Moreover, the synthesized bio-based flame retardant polyurethane is an intrinsic flame retardant polyurethane, and there is no need to add flame retardants to the bio-based flame retardant polyurethane, which solves the problems of large amount of flame retardant addition, easy precipitation, and low flame retardant efficiency in traditional flame retardant polyurethanes, and ensures the excellent mechanical properties of polyurethane.
[0025] The present invention uses the higher fatty acid monoester prepared from waste oil as raw material to prepare bio-based flame retardant polyol for the first time, which can not only effectively consume and utilize waste oil, but also be green and environmentally friendly; at the same time, the flame retardant prepared from the higher fatty acid monoester still maintains the plasticizing properties of the higher fatty acid monoester such as epoxy methyl ester after ring opening, and is added to polyurethane to significantly enhance its mechanical properties, and further improve the flame retardant effect. The higher fatty acid monoester has good compatibility with materials such as polyurethane, low volatility, good stabilization to light and heat, and can be applied to all polyvinyl chloride plastic products. Adding epoxy methyl ester can significantly improve the physical properties of the product and prolong the aging time, and has good synergistic effect when used with metal stabilizers such as barium, cadmium and zinc. Therefore, adding higher fatty acid alkyl ester into the flame retardant can enhance the fusion of the flame retardant and the material, so that it is not easy to precipitate and cause damage to the environment and material properties.
[0026] The higher fatty acid monoester prepared from waste oil in the present invention can also be directly purchased pure higher fatty acid monoester, which is added to polyurethane, and its flame retardant and mechanical properties will be further improved, but its cost will also be further increased.
[0027] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0028] The invention uses higher fatty acid monoester extracted from waste cooking oil as raw material, which is environmentally friendly, easily available and inexpensive. Using waste cooking oil as raw material for waste utilization greatly reduces costs and alleviates the difficulties in recycling and reusing waste cooking oil and the pollution to the environment.
[0029] The present invention uses epoxy ring-opening reaction as the core to prepare phosphorus-containing flame-retardant polyols. Compared with the traditional method of preparing flame-retardant polyols using phosphorus oxychloride and alcohol, the present invention requires simple conditions, does not require extra catalysts and solvents, and greatly reduces the preparation cost. The raw materials are easy to obtain, stable and less harmful to the human body. The hydroxyl structure of the polyol can be combined with polyurethane materials as a reactive flame retardant and is not easy to precipitate and cause damage to the environment.
[0030] The present invention is the first to use higher fatty acid monoesters prepared from waste oil as raw materials to prepare bio-based flame retardant polyols as flame retardants. Adding them into polyurethane can serve as both a flame retardant and a plasticizer, effectively improving the flame retardancy and mechanical properties of polyurethane products. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the infrared spectrum of the product of Example 1 of the present invention. DETAILED DESCRIPTION
[0032] The present invention is described in detail below with reference to specific embodiments.
[0033] The experimental methods described in the examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0034] Acid value determination method:
[0035] Use an analytical balance to weigh a certain amount of sample (0.2-0.5g) in a conical flask, add about 50mL of anhydrous ethanol, shake the conical flask thoroughly to dissolve the sample completely, and heat it if necessary, then add 1 drop of homemade phenolphthalein indicator, shake it evenly, and titrate it with 0.02mol / L KOH-CH3CH2OH standard titration solution to a blue color, and keep it at a non-fading position for 30s. Perform a blank test at the same time.
[0036] Calculation formula: Acid value (mgKOH·g -1 ) = (Vsample-Vspace) × c × 56.11 / m
[0037] Where Vsample - the amount of alkali standard solution used during sample titration, mL
[0038] Vblank——the amount of alkali standard solution used when titrating the blank sample, mL
[0039] c——Concentration of alkali standard solution, mol / L
[0040] m——sample mass, g
[0041] 56.11 – The specific value of the molar mass of potassium hydroxide, g / mol.
[0042] The preparation method of epoxy methyl ester in the embodiment of the present invention is according to the method in the existing literature, waste oil modification preparation of epoxy fatty acid methyl ester plasticizer for PVC, China Plastics, November 2014; wherein the epoxy fatty acid methyl ester plasticizer prepared in Section 1.3 is the epoxy methyl ester in the present invention, and the epoxy value of the prepared epoxy methyl ester reaches 3.9%, the iodine value is 8.70g / 100g, and the acid value is 6.5mgKOH / g. The preparation of other raw materials such as palmitoleic acid methyl ester, trans-linoleic acid methyl ester, stearic acid methyl ester, etc. can also refer to the above-mentioned literature or other literatures using waste oil as raw material for preparation. The above-mentioned can also directly use commercially available epoxy methyl ester, etc.
[0043] The anhydrous phosphoric acid in the examples is phosphoric acid with a purity of 99%.
[0044] Example 1
[0045] Weigh 5g of anhydrous phosphoric acid and place it in a four-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser. Use a constant pressure dropping funnel to add 14.74g of epoxy methyl ester. Control the liquid temperature to 70°C. After the addition is completed, keep the temperature at 70°C for 4h. Then add propylene oxide dropwise in three batches, 6.00g per batch, keep the temperature at 90°C for 2h each time, remove excess propylene oxide by vacuum distillation, and prepare epoxy methyl ester polyol. The acid value of the final product is 1.04mg KOH / g.
[0046] Example 2
[0047] Referring to Example 1, 5 g of anhydrous phosphoric acid was weighed and placed in a four-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser, and 14.74 g of epoxy methyl ester was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C, and after the addition was completed, the reaction was kept at 90°C for 4 hours. Then propylene oxide was added dropwise in three batches, 6.00 g per batch, and kept at 90°C for 2 hours each time. Excess propylene oxide was removed by vacuum distillation to prepare epoxy methyl ester polyol, and the acid value of the final product was 0.95 mg KOH / g.
[0048] Example 3
[0049] Referring to Example 1, 5 g of anhydrous phosphoric acid was weighed and placed in a four-necked flask equipped with stirring, a thermometer, and a condenser, and 44.22 g of epoxy methyl ester was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C, and after the addition was completed, the reaction was kept at 90°C for 4 hours. Then, 6 g of propylene oxide was added dropwise using a constant pressure dropping funnel three times, and each time the temperature was kept at 90°C for 2 hours. The excess propylene oxide was removed by vacuum distillation to prepare epoxy methyl ester polyol, and the acid value of the final product was 0.40 mgKOH / g. In this embodiment, the amount of epoxy methyl ester was increased to effectively reduce the acid value.
[0050] The infrared spectrum of the product prepared in this example is as follows Figure 1 In the infrared spectrum of epoxymethyl ester, 3460cm -1 The absorption peak at 2930cm is the vibration absorption peak of -OH, which may be caused by the residual glycerol; -1 、2855cm -1 1740cm -1 It is the C=O stretching vibration absorption peak of ester in fatty acid; 833cm -1 The absorption peak of epoxy group is at 833cm. -1 The absorption peak of epoxy group at 1020cm -1 The absorption peak at 1140 cm -1 The absorption peak is P=O. The above results show that epoxy methyl ester undergoes a ring-opening reaction with phosphoric acid, and the phosphate group is introduced into the long chain of soybean oil methyl ester.
[0051] Example 4
[0052] Referring to Example 1, 5 g of anhydrous phosphoric acid was weighed and placed in a four-necked flask equipped with a stirrer, a thermometer, and a condenser, and 44.22 g of epoxy methyl ester was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C, and after the addition was completed, the reaction was kept at 90°C for 4 hours. Then, 2.96 g of epichlorohydrin was added dropwise three times using a constant pressure dropping funnel, and each time the temperature was kept at 90°C for 3 hours. The excess epichlorohydrin was removed by reduced pressure distillation to prepare epoxy methyl ester polyol, and the acid value of the final product was 0.55 mgKOH / g.
[0053] Example 5
[0054] Referring to Example 1, 5 g of anhydrous phosphoric acid and 20 g of 1,4-dioxane were weighed and placed in a four-necked flask equipped with mechanical stirring, a thermometer, and a condenser, and 44.22 g of epoxy methyl ester was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C. After the addition was completed, the reaction was kept at 90°C for 4 hours. Then, 2.96 g of epichlorohydrin was added dropwise three times using a constant pressure dropping funnel, and each time the temperature was kept at 90°C for 3 hours. The excess epichlorohydrin was removed by vacuum distillation to prepare epoxy methyl ester polyol, and the final product acid value was 0.45 mgKOH / g. In this embodiment, the solvent 1,4-dioxane was added to make the phosphoric acid more dispersed. The reaction was more uniform and the acid value was lower.
[0055] Example 6
[0056] Example 6 adopts the method of Example 3, replacing anhydrous phosphoric acid with pyrophosphoric acid.
[0057] Example 7
[0058] Referring to Example 1, 5 g of anhydrous phosphoric acid and 20 g of 1,4-dioxane were weighed and placed in a four-necked flask equipped with a mechanical stirrer, a thermometer, and a condenser, and 40.26 g of methyl palmitoleate was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C, and after the addition was completed, the reaction was kept at 90°C for 4 hours. Then, 2.96 g of epichlorohydrin was added dropwise three times using a constant pressure dropping funnel, and each time the temperature was kept at 90°C for 3 hours, and the excess epichlorohydrin was removed by reduced pressure distillation. The acid value of the final product was 0.48 mgKOH / g.
[0059] Example 8
[0060] Referring to Example 1, 5 g of anhydrous phosphoric acid was weighed and placed in a four-necked flask equipped with a stirrer, a thermometer, and a condenser, and 44.25 g of methyl linoleate was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C, and after the addition was completed, the reaction was kept at 90°C for 4 hours. Then, 6 g of propylene oxide was added dropwise using a constant pressure dropping funnel three times, and the temperature was kept at 90°C for 2 hours each time. The excess propylene oxide was removed by reduced pressure distillation, and the acid value of the final product was 0.50 mgKOH / g.
[0061] Example 9
[0062] Referring to Example 1, 5 g of anhydrous phosphoric acid was weighed and placed in a four-necked flask equipped with a stirrer, a thermometer, and a condenser, and 44.77 g of methyl stearate was added using a constant pressure dropping funnel. The liquid temperature was controlled at 90°C, and after the addition was completed, the reaction was kept at 90°C for 4 hours. Then, 6 g of propylene oxide was added dropwise using a constant pressure dropping funnel three times, and each time the temperature was kept at 90°C for 2 hours. The excess propylene oxide was removed by reduced pressure distillation, and the acid value of the final product was 0.51 mgKOH / g.
[0063] Example 10
[0064] Application of higher fatty acid monoester polyols in polyurethane foam
[0065] The raw materials for preparing the polyurethane foam are all commercially available raw materials, and the method is also a conventional polyurethane preparation method.
[0066] Among them: PPG 4110 (polyether 4110 polyether polyol) was purchased from Jining Huakai Resin Co., Ltd.; DBTDL (dibutyltin dilaurate, product number D100274) was purchased from Aladdin Co., Ltd.;
[0067] TEOA (triethanolamine, item number T478536) was purchased from Aladdin Co., Ltd., AK 8805 (polyurethane foam stabilizer AK 8805) was purchased from Jiangsu Meside Chemical Co., Ltd.; n-hexane (normal hexane) was purchased from Shanghai Lingfeng Chemical Reagent Co., Ltd., PR (epoxy methyl ester flame retardant polyol prepared in Example 3 of the present invention).
[0068] Table 1 Formulation of flame retardant polyurethane foam
[0069] Samples PU-0 PU-P / 10 PU-P / 18 PU-P / 25 PPG 4110(g) 60 60 60 60 Water(g) 0.6 0.6 0.6 0.6 DBTDL(g) 1.5 1.5 1.5 1.5 TEOA(g) 0.3 0.3 0.3 0.3 AK 8805(g) 1.2 1.2 1.2 1.2 n-hexane(g) 6 6 6 6 PR(g) 0 7.2 15.6 24 PR(wt%) 0 10 18 25 Isocyanate index 1.2 1.2 1.2 1.2
[0070] The formula of the polyurethane composite material is shown in Table 1. The R (R = -NCO / -OH) of the PU composite material is 1.2. First, polyol, water, n-hexane, dibutyltin dilaurate (DBTDL), triethanolamine (TEOA), AK8805 (silicone oil, polyurethane foam stabilizer) and the flame retardant PR prepared in Example 3 are fully mixed in a plastic beaker at a speed of 1000 rpm for 10 minutes to form a uniform mixture, and isocyanate is added to make the isocyanate index 1.2, and stirred at a speed of 1500 rpm for 10s. Then the mixture is allowed to foam freely in a plastic cup and cured at room temperature for 72h. Finally, the PU composite material is cut into standard sizes for testing.
[0071] Test Standards
[0072] (1) Limiting oxygen index test
[0073] The limiting oxygen index (LOI) is an important indicator to measure the difficulty of material combustion. The larger the value, the more oxygen is required for the material to burn, the more difficult the material is to burn, and the better the flame retardant performance. According to ASTM D2863-97, the limiting oxygen index test was performed using a JF-3 HC-2C instrument (Jiangning, China). The sample size is 100×10×10mm 3 .
[0074] (2) Compression strength test
[0075] According to ASTM D1621, the compressive strength test of the samples was carried out, and the sample size was 50×50×25mm 3 , the deformation amount is 10%.
[0076] To evaluate the flammability of PU composites, the LOI and UL-94 test results of PU composites are listed in Table 2. The LOI value of PU-0 is 20.0%, which failed the UL-94 test and had a droplet phenomenon. The high flammability of PU-0 is due to the large specific surface area and porous structure of polyurethane. After the flame retardant prepared by the present invention was added to the material, the LOI value of PU-P continued to increase. When the flame retardant addition amount was 10-25wt%, the LOI value of PU-P increased from 23.7% to 26.2%, and the effect was very significant.
[0077] Table 2 LOI and UL-94 results of PU composites
[0078]
[0079] In order to evaluate the mechanical properties of PU composite materials, the compressive strength of PU composite materials is listed in Table 3. Compared with PU-0 without adding flame retardant, after adding flame retardant (PR), the compressive strength of polyurethane is increased from 0.130MPa to 0.265MPa, and the mechanical properties of polyurethane foam are significantly improved. In fact, adding flame retardant to polyurethane foam will affect the mechanical properties of polyurethane foam, and the more flame retardant is added, the greater the effect on the mechanical properties. The addition of many flame retardants in the prior art will lead to a decrease in the mechanical properties (such as compressive strength) of polyurethane foam (see Table 4 for details), and the more the amount added, the lower the strength, such as PUF-30 is added with 30% flame retardant. The specific flame retardant prepared by the present invention is added to polyurethane, which can significantly enhance its mechanical properties and further improve the flame retardant effect. The epoxy methyl ester flame retardant in the present invention has good compatibility with materials such as polyurethane, low volatility, good stabilization against light and heat, and can be applied to all polyvinyl chloride plastic products. It can significantly improve the physical properties of the products and prolong the aging time. When used in combination with metal stabilizers such as barium, cadmium and zinc, it has a good synergistic effect.
[0080] Table 3 Compressive strength results of PU composite materials
[0081] Samples Compressive Strength(MPa) PU-0 0.130 PU-P / 10 0.230 PU-P / 18 0.248 PI-P / 25 0.275
[0082] Table 4 Effect of flame retardant addition on mechanical properties of polyurethane foam in the prior art
[0083]
[0084] Reference 1: Preparation and Properties of Flame Retardant Soybean Oil-Based Polyurethane Rigid Foam, Huang Shizhao, Master’s Thesis of Hubei University, May 2019.
[0085] Reference 2: Synthesis of triazine ring-containing polyols and their application in polyurethane, Xu Shaoshuai, Master’s thesis of Hubei University, May 2020.
[0086] Reference 3: Research on flame retardant polyurethane rigid foam, Feng Yuelan, Chemical Propellants and Polymer Materials, Vol. 14, No. 4, 2016.
[0087] Reference 4: Preparation and Properties of Flame Retardant Rigid Polyurethane Foam Plastics, Liu Fengjiao, Master’s Thesis, Beijing University of Chemical Technology, June 2014.
Claims
1. A method for preparing a flame retardant polyol of a higher fatty acid monoester using waste oil as a raw material, characterized in that: The method comprises the following steps: adding higher fatty acid monoester and epoxy compound into phosphoric acid-containing compound to react and obtain higher fatty acid monoester polyol; the phosphoric acid-containing compound is anhydrous phosphoric acid or pyrophosphoric acid.
2. The method for preparing a flame retardant polyol of a higher fatty acid monoester using waste oil as a raw material according to claim 1, characterized in that: The anhydrous phosphoric acid is phosphoric acid with a purity of greater than or equal to 98%.
3. The method for preparing a flame retardant polyol of a higher fatty acid monoester using waste oil as a raw material according to claim 1, characterized in that: The higher fatty acid monoester is derived from treated waste cooking oil, and the higher fatty acid monoester includes any one or more of epoxy methyl ester, palmitoleic acid methyl ester, trans-linoleic acid methyl ester, and stearic acid methyl ester.
4. The method for preparing higher fatty acid monoester polyols using waste oil as raw material according to claim 1, characterized in that: The epoxy compound is preferably one or more of ethylene oxide, propylene oxide, epichlorohydrin, monohaloethylene oxide, monohalopropylene oxide, dihaloethylene oxide, and dihalopropylene oxide.
5. The method for preparing higher fatty acid monoester polyols using waste oil as raw material according to claim 1, characterized in that: The molar ratio of the phosphoric acid-containing compound, the higher fatty acid monoester and the epoxy compound is 1:0.5-3:1.5-8.
6. The method for preparing higher fatty acid monoester polyols using waste oil as raw material according to claim 1, characterized in that: The phosphoric acid-containing compound is placed in a reaction device, and after adding higher fatty acid monoester and epoxy compound, the reaction is kept warm until the reaction is completed.
7. The method for preparing higher fatty acid monoester polyols using waste oil as raw material according to claim 1, characterized in that: Add higher fatty acid monoesters and epoxy compounds, and keep warm at 25-100°C for 1-10 hours.
8. A higher fatty acid monoester polyol prepared by the method for preparing a higher fatty acid monoester polyol using waste cooking oil as a raw material as claimed in claim 1.
9. The higher fatty acid monoester polyol according to claim 8, characterized in that The higher fatty acid monoester polyol is a colorless or light yellow viscous oligomeric phosphoric (phosphonic) ester phosphoric acid containing one or two or more -P(O)OH structures in the middle of the chain.
10. Use of the higher fatty acid monoester polyol according to claim 1 as a flame retardant in the preparation of highly flame-retardant polyurethane foam plastics.
Citation Information
Patent Citations
Method for preparing epoxidized soybean oil with high epoxy value by fractional step method
CN101691524A
Method for synthesizing soybean oil-base polyether polyol
CN102250339A
Flame-retardant biomass polyalcohol as well as preparation method and application thereof
CN106632944A
Preparation method and applications of polyhydroxy phosphate
CN107445985A
Method for preparing reaction type flame-retardant polyether glycol through epoxidized soybean oil phosphorylation