Preparation method of biomass phosphonamide flame retardant and application of biomass phosphonamide flame retardant in PA6 / ABS (Polyamide 6 / Acrylonitrile Butadiene Styrene) alloy

By using new bio-based phosphonamide flame retardant in PA6/ABS alloy, the flame retardant performance and toughness are improved, the problems of insufficient flame retardant performance and environmental friendliness in the prior art are solved, and efficient flame retardant durability and The mechanical properties are balanced and meet the requirements of sustainable development.

CN118930580APending Publication Date: 2024-11-12禾欣可乐丽超纤皮(嘉兴)有限公司 +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410856712.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The flame retardant performance of existing PA6/ABS alloys is insufficient, the flame retardant has environmentally friendly problems, mechanical properties are degraded, and the impact strength is limited, which cannot meet the needs of high toughness and sustainable development.

Method used

Using a combination of a new bio-based phosphonamide flame retardant and PA6/ABS alloy, the flame retardant performance is improved and the long-term flame retardant performance is maintained while maintaining mechanical properties. Bio-based phosphonamide and PA6 compatibility and intermolecular hydrogen bonding inhibit surface migration.

Benefits of technology

It realizes the high flame retardant, high toughness and flame retardant durability of PA6/ABS alloy, improves impact strength, meets sustainable development requirements, and is easy to industrially produce.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930580A_ABST
    Figure CN118930580A_ABST
Patent Text Reader

Abstract

The invention discloses a biomass phosphonamide flame retardant, a preparation method thereof and an application of the biomass phosphonamide flame retardant in PA6 / ABS (Polyamide 6 / Acrylonitrile Butadiene Styrene) alloy. The flame-retardant PA6 composite material is prepared from the following components in parts by mass: 50 to 65 parts of PA6, 10 to 30 parts of ABS (Acrylonitrile Butadiene Styrene) and 5 to 25 parts of a bio-based phosphonamide flame retardant, 0.3 to 0.9 part of an antioxidant; 0.3 to 0.6 part of a lubricant; 2-10 parts of a flexibilizer and 1-5 parts of a compatilizer are used for preparing a flame-retardant nylon 6 composition; the biomass phosphonamide flame retardant is prepared by reacting phosphonyl chloride and bio-amine 3-aminopyridine. The biomass phosphoramide flame retardant prepared by the invention is high in compatibility with PA6 / ABS and good in flame retardant property, the flame retardant property of a PA6 / ABS alloy product can be remarkably improved, high impact strength up to 48 MJ / m < 2 > can be realized by matching with a proper toughening formula system, in addition, long-acting flame retardant property is maintained, and the application of the PA6 / ABS alloy in related fields can be well met and widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer alloy materials, and particularly relates to a biomass phosphamide flame retardant and a preparation method thereof and application thereof in PA6 / ABS alloy. Background Art

[0002] Polycaprolactam, also known as nylon 6 (PA6), is a typical aliphatic polyamide material. It is widely used in engineering plastics and film fields due to its excellent mechanical properties, chemical resistance and self-lubricating properties. However, PA6 has a low impact strength and cannot be directly used in scenarios with high toughness requirements. Therefore, using PA6 and ABS to prepare high-performance PA6 / ABS alloys is an important way to meet its application in related fields.

[0003] The flame retardant properties of the existing PA6 / ABS alloy need to be further improved. At the same time, most of the flame retardants used are halogen flame retardants, which are not environmentally friendly. Long-term use also causes surface migration, which leads to a decrease in flame retardant properties. At the same time, the mechanical properties decrease after adding flame retardants. In addition, these flame retardants are all derived from petroleum-based compounds, which do not comply with current sustainable development policies. Second, the impact strength of the current PA6 / ABS alloy remains at 20MJ / m 2 , its use is subject to certain restrictions. In order to solve the above problems, a new type of efficient biomass flame retardant and its high performance flame retardant PA6 / ABS alloy composite are developed to meet the current market demand. Summary of the invention

[0004] In order to prepare high-performance PA6 / ABS alloy materials, the present invention provides a PA6 / ABS alloy composition with flame retardancy, high toughness and flame retardancy durability. The present invention also provides a preparation method of a novel biomass phosphamide flame retardant. The use of the novel bio-based phosphamide flame retardant can improve the flame retardancy of the PA6 / ABS alloy and maintain long-lasting flame retardancy.

[0005] In the first aspect, the present invention provides a PA6 / ABS alloy having flame retardancy, high toughness and flame retardancy durability, which comprises the following components, in parts by mass: PA6 (50-65 parts), ABS resin (10-30 parts), bio-based phosphamide flame retardant (5-25 parts); antioxidant (0.3-0.9 parts); lubricant (0.3-0.6 parts); toughening agent (2-10 parts), and compatibilizer (1-5 parts).

[0006] Furthermore, the Mooney viscosity of the PA6 is between 2.0 and 2.5.

[0007] Furthermore, the ABS resin is a high-toughness ABS resin with a rubber content of more than 50%.

[0008] Furthermore, the bio-based phosphamide flame retardant has the structural formula:

[0009]

[0010] In the formula, R1 is selected from phenyl, phenoxy, 1-morpholinyl, di-1-adamantyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclononyl and cyclodecyl.

[0011] Furthermore, in the above formula, R1 is preferably phenyl, phenoxy or cyclohexyl.

[0012] Furthermore, the antioxidant is one or a combination of two of the commercially available antioxidants 9701, 1010, 1076, 168, 246, 300, and BHT.

[0013] Furthermore, the lubricant is at least one of PETS (pentaerythritol stearate), PE wax, silicone powder, and stearate.

[0014] Furthermore, the toughening agent is one of MBS (methyl methacrylate-butadiene-styrene graft copolymer), POE grafted MAH, polyolefin elastomer, MAH, and EMA.

[0015] Furthermore, the compatibilizer is at least one of styrene grafted maleic anhydride, styrene grafted GMA, and ethylene-butyl acrylate grafted GMA.

[0016] In a second aspect, the present invention provides a method for preparing a PA6 / ABS alloy having flame retardancy, high toughness and flame retardancy durability, which specifically comprises the following steps:

[0017] T1. Weigh the PA6, ABS, bio-based phosphamide flame retardant, antioxidant, lubricant, toughening agent, and compatibilizer according to the mass fraction;

[0018] T2. The above mixture was placed in a high-speed mixer for 4 minutes, with the stirring speed set to 300 rpm and the feed tray speed set to 50 rpm.

[0019] T3. Add the mixed raw materials into the twin-screw extruder and set the extruder parameters to the preset values.

[0020] T4. Start the twin-screw extruder, dryer and pelletizer for extrusion granulation.

[0021] T5. Dry the prepared PC / ABS alloy slices in a vacuum drying oven.

[0022] Furthermore, in step T3, the extruder parameters are as follows: the temperatures in the temperature control zones are 215° C., 235° C., 245° C., 245° C., 245° C., 245° C., 245° C., 245° C., 245° C., and 245° C., respectively, and the die head temperature is 255° C. The screw speed is 400 rpm, and the discharge rate is 35 kg / h.

[0023] Furthermore, in step T5, the drying temperature is 80-100° C. and the drying time is 4-6 hours.

[0024] In a third aspect, the present invention provides a method for preparing a bio-based phosphamide flame retardant, which is mainly prepared by reacting phosphonyl chloride and bio-based amine 3-aminopyridine.

[0025] Further, the molar ratio of the phosphinyl chloride to the bio-based amine 3-aminopyridine is (1-1.5):1, preferably 1:1;

[0026] Furthermore, the method specifically includes the following steps:

[0027] S1: dissolve phosphinoyl chloride in acetonitrile, add them into the reactor, and stir to dissolve at low temperature of -5-5℃;

[0028] S2: Dissolve the bio-based amine 3-aminopyridine and triethylamine in acetonitrile and add them dropwise into the reactor for reaction. The reaction time is 2-6 hours and the temperature is -10-5°C;

[0029] S3: heating to 40-80° C., reacting for 6-24 hours, filtering, washing and drying at 80-120° C. for 3-12 hours after the reaction to obtain the bio-based phosphamide flame retardant.

[0030] The excellent effect of adopting the above technical solution is that the temperature and time selected by the present invention are appropriate, which can reduce energy consumption and facilitate large-scale production.

[0031] Furthermore, the filtration is performed under normal pressure or under reduced pressure; the washing solvent is at least one of water, acetonitrile, tetrahydrofuran, benzene and toluene, preferably at least one of water, acetonitrile, benzene and toluene.

[0032] The beneficial effect of adopting the above further technical solution is that the present invention can directly remove the solvent by filtration, which is simple to operate and has a high yield.

[0033] Further, in step S1, the molar ratio of acetonitrile to phosphinoyl chloride is (2-15):1, preferably (2-3):1;

[0034] Furthermore, in step S2, the molar ratio of acetonitrile to 3-aminopyridine is (1-5):1, preferably (1-2):1; the molar ratio of triethylamine to the bio-based amine 3-aminopyridine is (1-6):1, preferably (1-3):1.

[0035] The beneficial effect of adopting the above further technical solution is that the molar ratio selected by the present invention can effectively inhibit the occurrence of side reactions, reduce the use of solvents, and is economical and effective.

[0036] Furthermore, the above-mentioned phosphinyl chloride is at least one of diphenylphosphinyl chloride, diphenyl chlorophosphate, dimorpholinyl phosphinyl chloride, di-1-adamantyl phosphinyl chloride, dicyclopropyl phosphinyl chloride, dicyclobutyl phosphinyl chloride, dicyclopentyl phosphinyl chloride, dicyclohexyl phosphinyl chloride, dicycloheptyl phosphinyl chloride, dicyclooctyl phosphinyl chloride, dicyclononyl phosphinyl chloride and dicyclodecyl phosphinyl chloride; preferably at least one of diphenylphosphinyl chloride, diphenyl chlorophosphate and dicyclohexyl phosphinyl chloride.

[0037] The beneficial effect of adopting the above further technical solution is that the phosphinoyl chloride selected by the present invention has high reaction activity and is easy to industrially produce.

[0038] The synthetic route of the above bio-based phosphamide flame retardant is:

[0039]

[0040] Furthermore, the reactor is purged with nitrogen before the reaction.

[0041] Furthermore, the reactor is provided with a reflux device for preventing the solvent from volatilizing during the temperature-raising reaction.

[0042] The beneficial effect of adopting the above further technical solution is that the selected bio-based amine 3-aminopyridine product process is relatively mature and has a positive effect on industrial production.

[0043] Beneficial effects of the present invention:

[0044] 1. The biomass phosphamide flame retardant prepared by the present invention contains a rigid ring structure, which gives the biomass phosphamide flame retardant itself excellent thermal stability and satisfies the processing requirements of PA6 / ABS alloy.

[0045] 2. The structure of the biomass phosphamide flame retardant prepared by the present invention is similar to the molecular chain structure of PA6, achieving good compatibility between the biomass phosphamide and the PA6 / ABS matrix, thereby maintaining good mechanical properties.

[0046] 3. The biomass phosphamide flame retardant prepared by the present invention forms intermolecular hydrogen bonds with PA6, thereby inhibiting the occurrence of surface migration and further maintaining the flame retardant durability of PA6 / ABS.

[0047] 4. The biomass phosphamide flame retardant of the present invention has a simple preparation method, a wide range of raw material sources, a high product yield, good flame retardant properties and is easy to industrialize, and can effectively improve the flame retardant properties of PA6 / ABS alloys. It has broad application prospects in various fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for describing the embodiment, wherein:

[0049] Figure 1 This is the infrared spectrum of the biomass phosphamide flame retardant prepared in Example 1;

[0050] Figure 2 The biomass phosphamide flame retardant prepared in Example 1 1 H NMR spectra;

[0051] Figure 3 The biomass phosphamide flame retardant prepared in Example 1 31 P NMR spectra;

[0052] Figure 4 This is the TGA chart of the biomass phosphamide flame retardant prepared in Example 1. DETAILED DESCRIPTION

[0053] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.

[0054] Embodiment 1:

[0055] Biomass phosphamide flame retardant, the structural formula is:

[0056]

[0057] The preparation method of the biomass phosphamide flame retardant specifically comprises the following steps: firstly dissolving 23.66g of diphenylphosphinyl chloride in 50mL of acetonitrile and adding the mixture into a 250mL four-mouth reactor with a nitrogen purge and reflux device, then dissolving 9.4g of 3-aminopyridine and 15.18g of triethylamine in 30ml of acetonitrile, then dripping the solution into the reactor drop by drop through a constant pressure dropping funnel, controlling the temperature to -5°C for reaction for 0.5h, then heating to 80°C for reaction for 3h, filtering under reduced pressure after the reaction is completed, washing with water, filtering, drying in a vacuum oven at 80°C for 6h to obtain a white solid powder, that is, obtaining the biomass phosphamide flame retardant.

[0058] The product was characterized by infrared spectroscopy, nuclear magnetic resonance hydrogen spectrum and nuclear magnetic resonance phosphorus spectrum. Figure 1 , Figure 2 and Figure 3 The thermal stability of the product was characterized, see Figure 4 .

[0059] Figure 1 This is the infrared spectrum of the biomass phosphamide flame retardant prepared in Example 1. Figure 1 It can be seen that the characteristic peaks of benzene ring, pyridine, PN and PC bonds appear in the figure. Figure 2 The following is the hydrogen nuclear magnetic resonance spectrum of the biomass phosphamide flame retardant prepared in Example 1. Figure 2 It can be seen that the integral of the proton number in the NMR spectrum is consistent with expectations. Figure 3 The NMR phosphorus spectrum of the biomass phosphamide flame retardant is shown in Figure 2. Figure 3 It can be seen that the NMR phosphorus spectrum contains only one chemical environment of phosphorus element. Figure 4 This is the TGA curve of the biomass phosphamide flame retardant prepared in Example 1. Figure 4 It can be seen that the prepared biomass phosphamide flame retardant has good thermal stability and can well meet the blending processing requirements of PA6 / ABS.

[0060] The synthetic route of the above biomass phosphamide flame retardant is as follows:

[0061]

[0062] Embodiment 2:

[0063] Biomass phosphamide flame retardant, the structural formula is:

[0064]

[0065] The preparation method of the biomass phosphamide flame retardant specifically comprises the following steps:

[0066] First, 26.86g of diphenyl chlorophosphate was dissolved in 60mL of acetonitrile and added into a 250mL four-mouth reactor with a nitrogen purge and reflux device, then 9.4g of 3-aminopyridine and 15.18g of triethylamine were dissolved in 50ml of acetonitrile, and then the solution was dripped into the reactor drop by drop through a constant pressure dropping funnel, the temperature was controlled to be 0°C for reaction for 3h, and then heated to 40°C for reaction for 12h, after the reaction was completed, the mixture was filtered under reduced pressure and washed with water, and after filtration, it was dried in a vacuum oven at a temperature of 100°C for 3h to obtain a white solid powder, that is, the biomass phosphamide flame retardant was obtained.

[0067] The synthetic route of the above biomass phosphamide flame retardant is as follows:

[0068]

[0069] Embodiment 3:

[0070] Biomass phosphamide flame retardant, the structural formula is:

[0071]

[0072] The preparation method of the biomass phosphamide flame retardant specifically comprises the following steps:

[0073] First, 24.85g of dicyclohexylphosphinoyl chloride is dissolved in 50mL of acetonitrile and added into a 250mL four-mouth reactor with a nitrogen purge and reflux device, then 9.4g of 3-aminopyridine and 15.18g of triethylamine are dissolved in 50ml of acetonitrile, and then the solution is dripped into the reactor drop by drop through a constant pressure dropping funnel, the temperature is controlled to be 0°C for reaction for 2h, and then heated to 80°C for reaction for 4h, after the reaction is completed, the mixture is filtered under reduced pressure and washed with water, and after filtration, it is dried in a vacuum oven at a temperature of 80°C for 6h to obtain a white solid powder, that is, the biomass phosphamide flame retardant is obtained.

[0074] The synthetic route of biomass phosphamide flame retardant is as follows:

[0075]

[0076] Embodiment 4:

[0077] The present embodiment provides a PA6 / ABS alloy with flame retardancy, high toughness and flame retardancy durability, which includes the following components in percentage by mass: PA6 resin (50%), ABS resin (27.4%), biomass phosphamide flame retardant (12%), antioxidant (0.3%), lubricant (0.3%), toughening agent (5%), and compatibilizer (5%).

[0078] Among them, PA6 resin (HS5000) was purchased from Jiangsu Hongsheng New Materials Co., Ltd., and the Mooney viscosity was 2.4.

[0079] The ABS resin (ABS757) was purchased from Chi Mei Industrial Co., Ltd. in Taiwan, China, and is a high-toughness ABS resin with a rubber content of more than 50%.

[0080] Wherein, the flame retardant is the biomass phosphamide flame retardant prepared in Example 1.

[0081] Among them, antioxidants 1010 and 168 were purchased from BASF (China) Co., Ltd. and compounded in a mass ratio of 1:1.

[0082] Among them, toughening agents WG-01 and EMA-200 were purchased from Coais Chemical and were compounded with polyolefin elastomer and EMA in a mass ratio of 1:1.

[0083] The compatibilizer is a compound of styrene grafted GMA and ethylene-butyl acrylate grafted EGMA, and is purchased from Quansheng Polycarbon Technology Co., Ltd.

[0084] The lubricant is pentaerythritol stearate (PETS), which is purchased from Luju Chemical.

[0085] The preparation method of the PA6 / ABS alloy with flame retardancy, high toughness and flame retardancy durability in this embodiment comprises the following steps:

[0086] According to the mass fraction, PA6 resin (50%), ABS resin (27.4%), biomass phosphamide flame retardant (12%), antioxidant (0.3%), lubricant (0.3%), toughening agent (5%), and compatibilizer (5%) were weighed and mixed in a high-speed mixer for 4 minutes. The stirring speed was set to 300 rpm and the feed plate speed was set to 50 rpm. After mixing, the mixture was added to a twin-screw extruder for extrusion granulation. The prepared PA6 / ABS alloy slices were dried in a vacuum drying oven at 80°C for 6 hours.

[0087] The parameters of the twin-screw extruder are as follows: the temperatures in the temperature control zones are 215°C, 235°C, 245°C, 245°C, 245°C, 245°C, 245°C, 245°C, and 245°C, respectively, and the die head temperature is 255°C. The screw speed is 400rpm, and the discharge capacity is 35kg / h.

[0088] Vertical combustion (UL-94) and oxygen index test: According to ASTM D2863-97 and ASTM D3801 standards, the composition is made into flame retardant test samples for testing by a flat plate vulcanizer. The temperature of the flat plate vulcanizer is set at 220-250°C, the vulcanization time is 1-5min, and the pressure is 10-25MPa.

[0089] Izod notched impact strength test: tested in accordance with GB / T 1591-2018 standard.

[0090] Tensile performance test: Tested in accordance with GB / T 1040.1-2018 standard

[0091] Bending performance test: Tested in accordance with GB / T 9341-2008 standard.

[0092] Tensile strength test results:

[0093] serial number Tensile strength(MPa) Elongation at break (%) Example 4 65 550

[0094] Bending strength test results:

[0095] serial number Bending strength(MPa) Flexural modulus (MPa) Example 4 100 2600

[0096] Flame retardant performance test results:

[0097] serial number UL-94(1.5mm) LOI(%) Example 4 VO 30

[0098] Izod notched impact strength test results:

[0099] serial number <![CDATA[Impact strength (MJ / m 2 )]]> Example 4 48

[0100] Flame retardant durability test: Boiling test: The test sample was placed in circulating hot water at 70°C, taken out after 168 hours, and then dried for performance test. The experimental results showed that the flame retardant grade was still V-0.

[0101] Embodiment 5:

[0102] The present embodiment provides a PA6 / ABS alloy with flame retardancy, high toughness and flame retardancy durability, which includes the following components in percentage by mass: PA6 resin (50%), ABS resin (27.4%), biomass phosphamide flame retardant (12%), antioxidant (0.3%), lubricant (0.3%), toughening agent (5%), and compatibilizer (5%).

[0103] Among them, PA6 resin (HS5000) was purchased from Jiangsu Hongsheng New Materials Co., Ltd. with a Mooney viscosity of 2.4.

[0104] The ABS resin (ABS757) was purchased from Chi Mei Industrial Co., Ltd. in Taiwan, China, and is a high-toughness ABS resin with a rubber content of more than 50%.

[0105] Among them, the flame retardant is the biomass phosphamide flame retardant prepared in Example 2.

[0106] Among them, antioxidants 1010 and 168 were purchased from BASF (China) Co., Ltd. and compounded in a mass ratio of 1:1.

[0107] Among them, toughening agents WG-01 and EMA-200 were purchased from Coase Chemical and were compounded from polyolefin elastomer and EMA.

[0108] The compatibilizer is a compound of styrene-grafted GMA and ethylene-butyl acrylate-grafted EGMA, and was purchased from Quansheng Polycarbon Technology Co., Ltd.

[0109] The lubricant is pentaerythritol stearate (PETS), which is purchased from Luju Chemical.

[0110] The preparation method of the PA6 / ABS alloy with flame retardancy, high toughness and flame retardancy durability in this embodiment comprises the following steps:

[0111] According to the mass fraction, PA6 resin (50%), ABS resin (27.4%), biomass phosphamide flame retardant (12%), antioxidant (0.3%), lubricant (0.3%), toughening agent (5%), and compatibilizer (5%) were weighed and mixed in a high-speed mixer for 4 minutes. The stirring speed was set to 300 rpm and the feed plate speed was set to 50 rpm. After mixing, the mixture was added to a twin-screw extruder for extrusion granulation. The prepared PA6 / ABS alloy slices were dried in a vacuum drying oven at 80°C for 6 hours.

[0112] The parameters of the twin-screw extruder are as follows: the temperatures in the temperature control zones are 215°C, 235°C, 245°C, 245°C, 245°C, 245°C, 245°C, 245°C, and 245°C, respectively, and the die head temperature is 255°C. The screw speed is 400rpm, and the discharge capacity is 35kg / h.

[0113] All test standards are consistent with those in the examples.

[0114] Tensile strength test results:

[0115] serial number Tensile strength(MPa) Elongation at break (%) Example 5 70 650

[0116] Bending strength test results:

[0117] serial number Bending strength(MPa) Flexural modulus (MPa) Example 5 95 2550

[0118] Flame retardant performance test results:

[0119] serial number UL-94(1.5mm) LOI(%) Example 5 V-2 33

[0120] Izod notched impact strength test results:

[0121] serial number <![CDATA[Impact strength (MJ / m 2 )]]> Example 5 46

[0122] Flame retardant durability test: Boiling test: The test sample was placed in circulating hot water at 70°C, taken out after 168 hours, and then dried for performance test. The experimental results showed that the flame retardant grade was still V-2.

[0123] Comparative Example 1:

[0124] Compared with Example 4, the biomass phosphamide flame retardant prepared in Example 1 was not added, and the rest of the preparation method was the same as that in Example 1 to obtain a PA6 / ABS alloy.

[0125] Tensile strength test:

[0126] serial number Tensile strength(MPa) Elongation at break (%) Comparative Example 1 58 500

[0127] Bending strength test:

[0128] serial number Bending strength(MPa) Flexural modulus (MPa) Comparative Example 1 90 2300

[0129] Flame retardant performance test:

[0130] serial number UL-94(1.5mm) LOI(%) Comparative Example 1 No rating 22

[0131] Izod notched impact strength test results:

[0132] serial number <![CDATA[Impact strength (MJ / m 2 )]]> Comparative Example 1 25

[0133] The present invention provides a PA6 / ABS alloy with flame retardancy, high toughness and flame retardancy durability. The present invention uses a novel biomass phosphamide flame retardant with a good toughening system and an appropriate ratio, and the flame retardancy grade can achieve 1.5mm, V-0 grade, and the cantilever beam notch impact strength reaches 48MJ / m2. In addition, the alloy still maintains the original flame retardancy and mechanical properties after boiling in 70 degrees Celsius for 168 hours. Flame retardant elements (phosphorus, nitrogen) and a rigid structure are introduced into the bio-phosphamide structure, giving the bio-based phosphamide flame retardant good thermal stability, the amide structure in the structure has good compatibility with the nylon 6 matrix, thereby maintaining the good mechanical properties of nylon 6, and the phosphamide melting point is below the processing temperature to achieve good compatibility in the alloy matrix. In addition, the NH bond in the bio-based phosphamide structure is used as a hydrogen bond donor and the C=O in the nylon 6 structure as a hydrogen bond acceptor to form an intermolecular hydrogen bond, which can well inhibit the surface migration of the bio-based phosphamide, thereby achieving good flame retardancy and durability. In addition, the flame retardant structure does not hydrolyze and has a high decomposition temperature. More importantly, the bio-based phosphamide is of biological origin and meets current sustainable development requirements.

[0134] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing a biomass phosphamide flame retardant, characterized in that: The following steps are involved: S1: dissolve phosphinoyl chloride in acetonitrile, add them into the reactor, and stir to dissolve at -5-5°C; S2: dissolving 3-aminopyridine and triethylamine in acetonitrile and adding dropwise into the reactor for reaction, the reaction time is 2-6h, the temperature is -10-5°C; S3: heating to 40-80° C., reacting for 6-24 hours, filtering, washing and drying at 80-120° C. for 3-12 hours after the reaction to obtain the biomass phosphamide flame retardant; The phosphinyl chloride is at least one of diphenylphosphinyl chloride, diphenyl chlorophosphate, dimorpholinylphosphinyl chloride, di-1-adamantylphosphinyl chloride, dicyclopropylphosphinyl chloride, dicyclobutylphosphinyl chloride, dicyclopentylphosphinyl chloride, dicyclohexylphosphinyl chloride, dicycloheptylphosphinyl chloride, dicyclooctylphosphinyl chloride, dicyclononylphosphinyl chloride and dicyclodecylphosphinyl chloride.

2. The method for preparing the biomass phosphamide flame retardant according to claim 1, characterized in that: The molar ratio of acetonitrile to phosphinoyl chloride in step S1 is (2-15):1; the molar ratio of acetonitrile to 3-aminopyridine in step S2 is (1-5):1, and the molar ratio of triethylamine to 3-aminopyridine is (1-6):

1.

3. The method for preparing the biomass phosphamide flame retardant according to claim 1, characterized in that: The molar ratio of acetonitrile to phosphinoyl chloride in step S1 is (2-3):1, the molar ratio of acetonitrile to 3-aminopyridine in step S2 is (1-2):1, and the molar ratio of triethylamine to 3-aminopyridine is (1-3):

1.

4. The biomass phosphamide flame retardant prepared by the preparation method according to claim 1 is characterized in that: The bio-based phosphamide flame retardant has the structural formula: In the formula, R1 is selected from one of phenyl, phenoxy, 1-morpholinyl, di-1-adamantyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclononyl and cyclodecyl.

5. Application of the biomass phosphamide flame retardant prepared by the preparation method according to claim 1 in PA6 / ABS alloy, characterized in that: The preparation method of the PA6 / ABS alloy is as follows: by weight, 0-65 parts of PA65, 10-30 parts of ABS resin, 5-25 parts of the biomass phosphamide flame retardant, 0.3-0.9 parts of antioxidant, 0.3-0.6 parts of lubricant, 2-10 parts of toughening agent and 1-5 parts of compatibilizer are mixed in a high-speed mixer, added into a twin-screw extruder, extruded, granulated and dried to obtain the PA6 / ABS alloy.

6. Application of the biomass phosphamide flame retardant prepared by the preparation method according to claim 5 in PA6 / ABS alloy, characterized in that: The parameters of the twin-screw extruder are set as: the temperatures in the temperature control zones are 215°C, 235°C, 245°C, 245°C, 245°C, 245°C, 245°C, 245°C, 245°C, respectively; the head temperature is 255°C, the screw speed is 400rpm, and the output is 35kg / h.

7. Application of the biomass phosphamide flame retardant prepared by the preparation method according to claim 5 in PA6 / ABS alloy, characterized in that: The antioxidant is one or a combination of two of the commercially available antioxidants 9701, 1010, 1076, 168, 246, 300 and BHT.

8. Application of the biomass phosphamide flame retardant prepared by the preparation method according to claim 5 in PA6 / ABS alloy, characterized in that: The Mooney viscosity of the PA6 is between 2.0 and 2.5; the ABS resin is a high-toughness ABS resin with a rubber content of more than 50%.

9. Application of the biomass phosphamide flame retardant prepared by the preparation method according to claim 5 in PA6 / ABS alloy, characterized in that: The lubricant is one of pentaerythritol stearate, polyethylene wax, silicone powder, and stearate; the toughening agent is one or more of methyl methacrylate-butadiene-styrene graft copolymer, POE grafted MAH, polyolefin elastomer, MAH, and EMA; the compatibilizer is at least one of styrene grafted maleic anhydride, styrene grafted GMA, and ethylene-butyl acrylate grafted GMA.

10. Application of the biomass phosphamide flame retardant prepared by the preparation method according to claim 5 in PA6 / ABS alloy, characterized in that: Calculated by weight, 50-60 parts of PA6, 25-28 parts of ABS resin, 12-14 parts of the biomass phosphamide flame retardant, 0.3-0.5 parts of antioxidant, 0.3-0.5 parts of lubricant, 4-6 parts of toughening agent and 3-5 parts of compatibilizer are mixed in a high-speed mixer, added into a twin-screw extruder, extruded, granulated and dried to obtain a PA6 / ABS alloy.