High-voltage direct-current cable insulating material capable of inhibiting high-temperature and high-field conductance and preparation method thereof
By using graft-modified crosslinked polyethylene technology in high-voltage DC cable insulation materials, the cross-linking reaction between polar compounds and polyethylene molecular chains is used to form a stable deep trap and hydrogen bond structure, and the conductivity current at high temperature and high fields is solved The problems of rapid growth and poor material stability have significantly improved the breakdown resistance and stability of insulating materials.
Patent Information
- Application Number
- CN202410957823.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
High-voltage DC cable cross-linked polyethylene insulating material grows rapidly under high temperature and high field strength. The electric field-temperature gradient coupling field causes the electric field to reverse, and small molecular compounds containing polar groups are easily migrated and precipitated, and modified insulating material Poor performance stability.
Using graft modified crosslinked polyethylene insulating material prepared from polyethylene, polar compounds and initiators, polar compounds are fixed by adding polar compounds to polyethylene and melt kneading and crosslinking reaction at high temperature. On the polyethylene molecular chain, a structure with deep traps and hydrogen bonds is formed, reducing the carrier mobility and conductivity current growth rate.
It effectively suppresses the conductivity current growth rate under high temperature and high fields, improves breakdown resistance and material stability, reduces the possibility of electric field inversion of the insulating layer, and extends the service life of the cable.
Smart Images

Figure CN118930740A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-voltage direct current cable insulating material capable of suppressing high-temperature and high-field conductivity and a preparation method thereof, belonging to the technical field of high-voltage direct current cables and preparation thereof. Background Art
[0002] Polyethylene insulated cables have excellent electrical properties and have been widely used in many fields such as high-voltage direct current transmission, new energy grid interconnection, submarine power transmission, etc. However, unlike AC transmission lines, the transmission loss of high-voltage direct current transmission lines is positively correlated with the conductivity of the insulation material. Higher conductivity will increase the leakage current, which will not only cause energy waste, but also release the loss in the form of internal energy, causing the cable insulation temperature to rise, accelerating insulation aging and even damaging the insulator, reducing the service life of the cable. At the same time, the internal electric field distribution of the cable insulation under the action of the high-voltage direct current electric field is controlled by the material conductivity and is inversely proportional to it, and the conductivity increases significantly with the increase of temperature. During the operation of the high-voltage direct current cable, the higher temperature of the core and the lower temperature of the sheath will cause a temperature gradient inside the insulation, resulting in the problem of electric field reversal under the action of the electric field-temperature gradient coupling field, causing the electric field on the outer surface of the insulation layer to be greater than the electric field on the inner surface of the insulation layer, reducing the safety and stability of the cable operation.
[0003] Studies have pointed out that the introduction of polar groups such as carbonyl, hydroxyl, nitro, cyano or aromatic rings into polyolefins can significantly inhibit the accumulation of charges in the material, effectively reduce the mobility of carriers inside the material, and reduce the growth rate of the conduction current of the insulating material under high temperature and high field strength. However, small molecule compounds containing polar groups are easy to migrate and precipitate during the production, storage and use of cables, and polar polymers have poor compatibility with polyolefins, thereby reducing the performance effect of polar compounds in inhibiting the growth rate of the conduction current of the insulating material under high temperature and high field strength, resulting in poor performance stability of the modified insulating material. Therefore, the present invention provides a graft-modified cross-linked polyethylene high-voltage DC cable insulating material that can inhibit high-temperature and high-field conductivity and a preparation method thereof. Summary of the invention
[0004] The present invention aims to solve the problems that the conductivity current of the existing high-voltage direct current cable cross-linked polyethylene insulation material increases rapidly under high temperature and high field strength, the electric field is reversed under the action of the electric field-temperature gradient coupling field, the small molecule compounds containing polar groups are easy to migrate and precipitate, and the performance stability of the modified insulation material is poor. The present invention provides a high-voltage direct current cable insulation material capable of suppressing high-temperature and high-field conductivity and a preparation method thereof.
[0005] The technical solution of the present invention:
[0006] A high-voltage DC cable insulating material capable of suppressing high-temperature and high-field conductivity, the insulating material being made of the following raw materials in parts by weight: 100 parts of polyethylene, 0.02 to 6 parts of an initiator and 0.05 to 10 parts of a polar compound;
[0007] The polar compound has an ethylenically unsaturated substituent.
[0008] It is further defined that the polar compound is an o-hydroxybenzophenone type ultraviolet absorber.
[0009] In a further embodiment, the polar compound is 2-hydroxy-4-(methacryloyloxy)benzophenone.
[0010] In a further embodiment, the initiator is DCP or BIPB.
[0011] It is further defined that the amount of initiator used is 0.03 to 4 parts.
[0012] It is further defined that the insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 2 parts of DCP and 0.5 parts of 2-hydroxy-4-(methacryloyloxy)benzophenone.
[0013] It is further defined that the insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 3 parts of DCP and 1 part of 2-hydroxy-4-(methacryloyloxy)benzophenone.
[0014] Further defined, the insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 1 part of BIPB and 0.5 parts of 2-hydroxy-4-(methacryloyloxy)benzophenone.
[0015] The second object of the present invention is to provide a method for preparing the above-mentioned high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity, the method comprising the following steps:
[0016] (1) adding polyethylene to a torque rheometer and then melting it, and then sequentially adding a polar compound and an initiator, and kneading for 3 to 30 minutes at a temperature of 80 to 130° C. and a rotation speed of 50 to 60 r / min to obtain a blend;
[0017] (2) The blend is placed in a flat vulcanizer, and is continuously pressurized to 10-25 MPa at 80-130° C. for melting and shaping for 15-40 minutes. After shaping, the blend is transferred to a flat vulcanizer at a temperature of 160-190° C. and directly pressurized to 10-25 MPa for cross-linking and grafting for 20-50 minutes to obtain a high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity.
[0018] Further defined, (1) is to add a polar compound to molten polyethylene, mix for 3 to 15 minutes at a temperature of 80 to 130° C. and a rotation speed of 50 to 60 r / min, then add an initiator, and continue mixing for 1 to 10 minutes to obtain a blend.
[0019] Beneficial effects of the present invention:
[0020] (1) The present invention adds polar compounds to polyethylene, triggers the polar compounds to bond to polyethylene molecular chains through melt grafting reaction, so that the polar compounds are fixed on the polyethylene molecular chains. At the same time, cross-linking reaction occurs between polyethylene macromolecules to generate polar compound grafted modified cross-linked polyethylene. Polar groups such as carbonyl and hydroxyl groups and benzene rings in polar compounds can introduce deep traps in cross-linked polyethylene, and polar compounds have high electron affinity, which makes polar compounds have a greater probability of capturing high-energy electrons, reducing the number and mobility of carriers inside the modified insulating material, thereby inhibiting the conductivity current growth rate of the cross-linked polyethylene insulating material under high temperature and high field strength.
[0021] (2) The ortho-hydroxyl group on the benzene ring in the polar compound used in the present invention and the carbonyl oxygen atom can form an intramolecular hydrogen bond chelate ring. Under the action of the electric field, the intramolecular structure undergoes thermal vibration, the intramolecular hydrogen bond is destroyed, the chelate ring is opened, and at the same time, the carbonyl group in the molecule is also excited, and the excited state intramolecular proton transfers to generate enol-quinone tautomers, and the intramolecular structure changes. In addition, the polar compound has a narrow energy gap. The change in molecular structure and the narrow energy gap enable the polar compound to release the absorbed energy in the form of internal energy, which is relatively less harmful. Therefore, after the polar compound is grafted and modified, the probability of the electrons inside the material bombarding the cross-linked polyethylene macromolecular chain is reduced, the destructive effect is greatly weakened, and the breakdown resistance is improved.
[0022] (3) The polar compound grafted on the cross-linked polyethylene molecular chain of the present invention is not easy to migrate or precipitate, has good compatibility with the cross-linked polyethylene, and has good stability in inhibiting the growth of the conductive current. Therefore, the polar compound grafted modified cross-linked polyethylene high-voltage DC cable insulation material prepared by the present invention has high breakdown resistance and the performance of the modified polar compound being stable and not easy to precipitate, on the basis of being able to inhibit the growth of the conductive current of the insulation material under high temperature and high field strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A reaction principle diagram for preparing a high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity according to the present invention;
[0024] Figure 2 The conductive current curves of the insulating materials prepared in Example 1 and Comparative Example 1 at different temperatures, where a is 30° C. and b is 90° C.;
[0025] Figure 3 The Weibull distribution diagram of the DC breakdown field strength of the insulating materials prepared in Example 1 and Comparative Example 1 at different temperatures, wherein a is 30° C. and b is 90° C.;
[0026] Figure 4 The conductive current curves of the insulating materials prepared in Example 2 and Comparative Example 1 at different temperatures, where a is 30°C and b is 90°C;
[0027] Figure 5 The Weibull distribution diagram of the DC breakdown field strength of the insulating materials prepared in Example 2 and Comparative Example 1 at different temperatures, wherein a is 30° C. and b is 90° C.;
[0028] Figure 6 The conductive current curves of the insulating materials prepared in Example 3 and Comparative Example 1 at different temperatures, where a is 30°C and b is 90°C;
[0029] Figure 7 The conductive current curves of the insulating materials prepared in Example 4 and Comparative Example 1 at different temperatures, where a is 30°C and b is 90°C; DETAILED DESCRIPTION
[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0031] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0032] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0033] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0034] Example 1
[0035] 40g of polyethylene was added to a torque rheometer and melted at a speed of 50r / min and 110°C. After it was melted, 0.2g of 2-hydroxy-4-(methacryloyloxy)benzophenone was added, and the mixture was kneaded at the same temperature and speed for 8min. Then, 0.8g of diisopropylbenzene peroxide was added, and the mixture was kneaded at the same temperature and speed for 5min to obtain a blend. The blend was then placed in a flat vulcanizer, and the pressure was increased from 0MPa to 5, 10, and 15MPa at 110°C to melt and shape for 30min. After the mixture was melted, it was transferred to a flat vulcanizer at a temperature of 175°C and directly pressurized to 15MPa for cross-linking and grafting for 30min to obtain a grafted modified cross-linked polyethylene high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity.
[0036] The reaction process of preparing the graft-modified cross-linked polyethylene high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity in this embodiment is as follows: Figure 1 As shown, the initiator diisopropylbenzene peroxide decomposes at high temperature to generate primary free radicals, which undergo hydrogen elimination reaction with polyethylene molecular chains to generate polyethylene macromolecular chain free radicals, which undergo addition reaction with polar compound 2-hydroxy-4-(methacryloyloxy)benzophenone monomer to generate graft free radicals and undergo hydrogen transfer, while cross-linking reaction occurs between graft free radicals and polyethylene macromolecular chain free radicals and between polyethylene macromolecular chain free radicals to generate cross-linked polyethylene, and finally generate polar compound grafted modified cross-linked polyethylene insulating material.
[0037] Example 2
[0038] 40g of polyethylene was added to a torque rheometer at a speed of 60r / min and melted at 120°C. After it was melted, 0.4g of 2-hydroxy-4-(methacryloyloxy)benzophenone was added, and the mixture was kneaded at the same temperature and speed for 5min. Then, 1.2g of diisopropylbenzene peroxide was added, and the mixture was kneaded at the same temperature and speed for 3min to obtain a blend. The blend was then placed in a flat vulcanizer, and the pressure was increased from 0MPa to 5, 10, 15, 20, and 25MPa at 120°C in sequence to melt and shape for 20min. After the mixture was completed, it was transferred to a flat vulcanizer at a temperature of 170°C and directly pressurized to 25MPa for cross-linking and grafting for 40min to obtain a grafted modified cross-linked polyethylene high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity.
[0039] Example 3
[0040] 40g of polyethylene was added to a torque rheometer at a speed of 55r / min and melted at 100°C. After it was melted, 0.2g of 2-hydroxy-4-(methacryloyloxy)benzophenone was added, and the mixture was mixed at the same temperature and speed for 10min. Then, 0.4g of di(tert-butylperoxyisopropyl)benzene was added, and the mixture was mixed at the same temperature and speed for 8min to obtain a blend. The blend was then placed in a flat vulcanizer, and the pressure was increased from 0MPa to 5, 10, 15, and 20MPa in sequence at 100°C for melting and shaping for 35min. After the mixture was finished, it was transferred to a flat vulcanizer at a temperature of 185°C and directly pressurized to 20MPa for cross-linking and grafting for 25min to obtain a grafted modified cross-linked polyethylene high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity.
[0041] Example 4
[0042] 40g of polyethylene was added to a torque rheometer at a speed of 55r / min and melted at 90°C. After it was melted, 0.4g of 2-hydroxy-4-(methacryloyloxy)benzophenone was added, and the mixture was mixed at the same temperature and speed for 15min. Then, 0.8g of di(tert-butylperoxyisopropyl)benzene was added, and the mixture was mixed at the same temperature and speed for 10min to obtain a blend. The blend was then placed in a flat vulcanizer, and the pressure was increased from 0MPa to 5, 10, 15, 20, and 25MPa at 90°C to melt and shape for 40min. After the mixture was melted, it was transferred to a flat vulcanizer at a temperature of 185°C and directly pressurized to 25MPa for cross-linking and grafting for 25min to obtain a grafted modified cross-linked polyethylene high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity.
[0043] Comparative Example 1
[0044] 40g of polyethylene was added to the torque rheometer at a speed of 50r / min, and melted at 110°C. After it was melted, 0.8g of diisopropylbenzene peroxide was added, and mixing was continued for 5min at the same temperature and speed to obtain a blend. The blend was then placed in a flat-plate vulcanizer, and the pressure was increased from 0MPa to 5, 10, and 15MPa at 110°C for melting and shaping for 30min. After the end, it was transferred to a flat-plate vulcanizer at a temperature of 175°C and directly pressurized to 15MPa for a cross-linking process of 30min to obtain pure cross-linked polyethylene high-voltage DC cable insulation material.
[0045] Effect example
[0046] (1) The conductance current of the insulating material samples obtained in Examples 1 to 4 and Comparative Example 1 was tested using a three-electrode system. The thickness of the sample was about 70 μm. The test temperature was 30° C. and 90° C. The applied field strength was 5, 10, 15, 20, 25, 30, 35, 40, 50, 60, 70, 80, 90, and 100 kV / mm, respectively. After the voltage was stable for 5 min at each field strength, the measurement was started. The test results were as follows: Figure 2 , 4 , 6 and 7 as shown.
[0047] contrast Figure 2 , Figure 4 , Figure 6 and Figure 7 The conductivity current curves of the insulating materials shown in the figure show that the polar compound grafted modified cross-linked polyethylene insulating materials prepared in Example 1, Example 2, Example 3 and Example 4 have better conductivity current suppression capabilities at different temperatures than the pure cross-linked polyethylene insulating material prepared in Comparative Example 1. Figure 2 (a) Figure 4 (a) Figure 6 (a) and Figure 7 (a) shows the conductivity current curve. Under low temperature conditions, the conductivity current density of the polar compound grafted cross-linked polyethylene insulation material is significantly reduced compared to the pure cross-linked polyethylene insulation material. With the increase of the electric field strength, the slope of the conductivity current curve of the polar compound grafted cross-linked polyethylene has a significant downward trend at higher field strengths, and with the increase of the polar compound content, the trend of the curve slope decreasing becomes more and more obvious. Figure 2 (b) Figure 4 (b) Figure 6 (b) and Figure 7 (b) shows that under high temperature conditions, the conductivity current density of the cross-linked polyethylene insulation material grafted with polar compounds is still lower than that of the pure cross-linked polyethylene insulation material, and under higher field strength, the slope of the conductivity current curve of the cross-linked polyethylene insulation material grafted with polar compounds also shows a decreasing trend. As the number of polar compounds increases, the trend of decreasing curve slope is still more and more obvious. It can be seen that the polar compound grafted cross-linked polyethylene high-voltage DC cable insulation material prepared in the above embodiment can effectively suppress the conductivity current growth rate under high temperature and high field strength, and shows better conductivity current suppression ability than pure cross-linked polyethylene insulation material, which can reduce the possibility of electric field reversal in the insulation layer, which will greatly improve the electrical properties of the insulation material.
[0048] (2) The DC breakdown strength of the insulating material samples obtained in Examples 1 to 2 and Comparative Example 1 was tested using a columnar two-electrode system. The thickness of the sample was about 70 μm. The test temperature was 30° C. and 90° C. The sheet sample was placed between the upper and lower electrodes and immersed in silicone oil. The sample was pressurized at a uniform speed until it broke down. After that, the breakdown voltage was read and the breakdown field strength was calculated. The data was processed using the Weibull distribution function. The test results are shown in FIG. Figure 3 and Figure 5 shown.
[0049] like Figure 3 and Figure 5 As shown, by comparing the breakdown field strength test results of the insulating materials obtained by Example 1, Example 2 and Comparative Example 1, it can be seen that the use of polar compound grafting can effectively improve the DC breakdown field strength of cross-linked polyethylene. The breakdown field strengths of the pure cross-linked polyethylene insulating material obtained in Comparative Example 1 and the polar compound grafted modified cross-linked polyethylene insulating material obtained by Example 1 and Example 2 are 307.1, 376.0 and 420.9 kV / mm at 30°C, respectively, and the breakdown field strengths at 90°C are 181.6, 182.9 and 188.7 kV / mm, respectively. With the increase of temperature, the breakdown field strengths of pure cross-linked polyethylene and polar compound grafted modified cross-linked polyethylene insulating materials are reduced. With the increase of the number of polar compounds, the breakdown field strength of the grafted modified cross-linked polyethylene insulating material gradually increases. Therefore, the breakdown resistance of the polar compound grafted modified cross-linked polyethylene high-voltage DC cable insulating material obtained in the above embodiments is significantly improved.
[0050] The above description is only a preferred embodiment of the present invention. In view of the fact that technicians in the field of the present invention can make appropriate changes and modifications to the above implementation, the present invention is not limited to the specific implementation described above. Some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention.
Claims
1. A high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity, characterized in that: The insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 0.02 to 6 parts of initiator and 0.05 to 10 parts of polar compound; The polar compound has an ethylenically unsaturated substituent.
2. The insulating material according to claim 1, characterized in that The polar compound is an o-hydroxybenzophenone type ultraviolet absorber.
3. The insulating material according to claim 2, characterized in that The polar compound is 2-hydroxy-4-(methacryloyloxy)benzophenone.
4. The insulating material according to claim 3, characterized in that The initiator is DCP or BIPB.
5. The insulating material according to claim 1, characterized in that The amount of initiator used is 0.03 to 4 parts.
6. The insulating material according to claim 4, characterized in that The insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 2 parts of DCP and 0.5 parts of 2-hydroxy-4-(methacryloyloxy)benzophenone.
7. The insulating material according to claim 4, characterized in that The insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 3 parts of DCP and 1 part of 2-hydroxy-4-(methacryloyloxy)benzophenone.
8. The insulating material according to claim 4, characterized in that The insulating material is made of the following raw materials in parts by weight: 100 parts of polyethylene, 1 part of BIPB and 0.5 parts of 2-hydroxy-4-(methacryloyloxy)benzophenone.
9. A method for preparing a high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity according to any one of claims 1 to 8, characterized in that: include: (1) adding polyethylene to a torque rheometer and then melting it, and then sequentially adding a polar compound and an initiator, and kneading for 3 to 30 minutes at a temperature of 80 to 130° C. and a rotation speed of 50 to 60 r / min to obtain a blend; (2) The blend is placed in a flat vulcanizer, and is continuously pressurized to 10-25 MPa at 80-130° C. for melting and shaping for 15-40 minutes. After shaping, the blend is transferred to a flat vulcanizer at a temperature of 160-190° C. and directly pressurized to 10-25 MPa for cross-linking and grafting for 20-50 minutes to obtain a high-voltage DC cable insulation material capable of suppressing high-temperature and high-field conductivity.
10. The preparation method according to claim 9, characterized in that: (1) After adding polar compounds to molten polyethylene, the mixture is kneaded for 3 to 15 minutes at a temperature of 80 to 130° C. and a rotation speed of 50 to 60 r / min, and then an initiator is added and kneaded for 1 to 10 minutes to obtain a blend.
Citation Information
Patent Citations
Crosslinked polyethylene cable insulating material containing compounding agent with high electrical resistance and preparation method thereof