High-barrier cycloolefin polymer and preparation method thereof
By introducing fluoroalkyl or fluoroaryl structures into cycloolefin polymers, a strong electronegative dense structure is formed, which solves the problem of insufficient oxygen resistance performance of cycloolefin polymers in the prior art, and achieves high barrier properties and high barrier properties Transparent polymers are suitable for packaging materials and have good recyclability.
Patent Information
- Application Number
- CN202411080699.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The existing high-barrier polymer materials have shortcomings in achieving high barrier properties to water and oxygen at the same time, especially the oxygen resistance performance of cycloolefin polymers has not been significantly improved, and the multi-layer composite or aluminum plating process is complicated and unfavorable. Material recycling.
Using a highly barrier cycloolefin polymer containing fluoroalkyl or fluoroaryl structural units, it is prepared by ring-opening metathesis polymerization and hydrogenation reaction to form a polymer with strong electronegative and dense structure, which improves its resistance. Water and oxygen resistance properties while maintaining high transparency.
High-transparent and high heat resistance are achieved, which significantly reduces the transmission of water vapor and oxygen, takes into account the optical properties of the material, and provides more environmentally friendly recycling.
Smart Images

Figure BDA0004983646770000021 
Figure BDA0004983646770000022 
Figure BDA0004983646770000023
Abstract
Description
Technical Field
[0001] The invention relates to the field of polyolefins, and in particular to a high-barrier cycloolefin polymer and a preparation method thereof. Background Art
[0002] High barrier polymer materials are materials with special functions. They have "high barrier" characteristics and low permeability to low molecular weight chemicals such as water vapor and oxygen. Due to their barrier properties, when they are made into films and used in food packaging (especially meat processing products, raw meat, cheese, salad dressing, sauces, agricultural products and seafood processing products), they can prevent the oxidation and microbial growth caused by the penetration of oxygen and other gases, and prevent the outflow of fragrance, soup, etc., thereby improving the storage of the contents. In addition, high barrier polymer films should also have strong water vapor barrier properties to prevent the contents from becoming moldy due to the penetration of water vapor.
[0003] The existing high barrier polymers are mostly polyolefin materials such as PE, PP, PVC, PET polyester, PA nylon, EVOH and other materials. Among them, polyolefin materials such as PE and PP have excellent water barrier properties, but the interaction between molecular chains is weak and the oxygen barrier properties are average. PA nylon materials, EVOH and other materials have a large number of hydrogen bonds between molecular chains, which makes them have excellent oxygen barrier properties, but the presence of polar groups makes their water barrier properties average.
[0004] In order to achieve high barrier properties to both water and oxygen, the existing technical solutions are: (1) multi-layer composite of polyolefin materials with excellent water barrier properties and nylon, EVOH and other materials with excellent oxygen barrier properties; (2) aluminum plating on polyolefin substrates to improve barrier properties. In these two solutions, in addition to the need to introduce complex multi-layer co-extrusion film-forming processes or high-temperature aluminum plating processes, other components other than polyolefin are introduced into the product. When recycling the materials, different composite layers need to be peeled off, which makes it difficult to achieve quick recycling and brings serious environmental burdens.
[0005] Cyclic olefin polymer (COP) is an amorphous transparent high molecular polymer with a high sterically hindered cyclic alkane structure on the main chain of the molecule. It is prepared by ring-opening metathesis polymerization of cycloolefins and then hydrogenation. Currently, commercialized COP materials include ZEONEX and ZEONOR of Japan's ZEON Company, and ARTON of Japan's JSR Company. Due to the excellent properties of COP materials such as good light transmittance, good molding processability, and low hygroscopicity, COP is widely used in polarizers, medical treatment, packaging materials and other fields. Among them, ZEONEX and ZEONOR series COP products of ZEON are composed of pure C and H elements. Their water barrier properties are better than those of polyolefin packaging materials such as PE and PP. When blended with PE and PP, they can improve the water barrier properties of PE and PP, but the oxygen barrier properties have not been significantly improved. Therefore, improving the oxygen barrier properties of COP is still the direction for improving materials. Summary of the invention
[0006] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a high barrier cycloolefin polymer having both oxygen barrier and water barrier properties and a preparation method thereof. The high barrier cycloolefin polymer of the present invention has the characteristics of high transparency and high heat resistance in addition to barrier properties.
[0007] In order to achieve the above technical effects, the present invention adopts the following scheme:
[0008] In a first aspect, the present invention provides a high barrier cycloolefin polymer comprising a structural unit as shown in the following formula I:
[0009]
[0010] In formula I, L is -CH2-CH2- or -CH=CH-; n is an integer from 0 to 2; R is a fluoroalkyl group or a fluoroaryl group, preferably a fluoroalkyl group such as trifluoromethyl, pentafluoroethyl, heptafluoropropyl, or one or more fluoroaryl groups such as trifluorophenyl and pentafluorophenyl; and x is 10-500.
[0011] In some preferred embodiments, the high barrier cycloolefin polymer of the present invention further comprises a structural unit as shown in the following formula II:
[0012]
[0013] In Formula II, RC is any one of an alkyl group and a cycloalkyl group, preferably a C4-C8 alkyl group, a C5-C 15 Any of the cycloalkyl groups of C4-C8, more preferably C4-C8 alkylene groups, C5-C 15 Any one of the groups containing a cyclopentane structure; y is 50-500.
[0014] In some preferred embodiments, the high barrier cycloolefin polymer described in the present invention has a combination of blocks of structural units shown in formula I and blocks of structural units shown in formula II, and the total number of blocks of the structural units shown in formula I and the blocks of the structural units shown in formula II is 2-5.
[0015] In some preferred embodiments, the structural unit represented by formula I of the present invention is prepared by ring-opening polymerization of the compound represented by formula I-A under the action of a chain transfer agent:
[0016]
[0017] In formula Ⅰ-A, R and n are defined the same as R and n in the above formula Ⅰ;
[0018] Preferably, the compound represented by formula Ⅰ-A is selected from at least one of compounds M-1, M-2, M-3, M-4, and M-5 having the following structures:
[0019]
[0020] In some preferred embodiments, the structural unit represented by formula II of the present invention is prepared by a cycloolefin compound represented by formula II-A:
[0021]
[0022] Wherein, the definition of RC is the same as that of RC in the above formula II;
[0023] Preferably, the cycloolefin compound represented by formula II-A is at least one selected from cyclopentene, cyclohexene, cycloheptene, cyclooctene, cyclooctadiene, norbornene, dicyclopentadiene and tetracyclododecene.
[0024] In the present invention, the high barrier cycloolefin polymer has a number average molecular weight of 5000-100000, for example, 5000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 100000.
[0025] In the present invention, the high barrier cycloolefin polymer has a double bond molar content of ≤50%, such as 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 1%, preferably ≤1%.
[0026] In the present invention, the high barrier cycloolefin polymer has a water vapor transmission rate of <1g / (m 2 .24h);
[0027] In the present invention, the high barrier cycloolefin polymer has an oxygen permeability of 50-100cm2 under GB / T1038 standard. 3 / (m 2 .24h.0.1MPa);
[0028] In the present invention, the high barrier cycloolefin polymer has a visible light transmittance of 89%-93% under GB / T2410 standard;
[0029] In a second aspect, the present invention further provides a method for preparing the above-mentioned high barrier cycloolefin polymer. The method for preparing olefin polymer is well known to those skilled in the art. The following is only an exemplary description and does not constitute any limitation.
[0030] For example, a method for preparing the above-mentioned high barrier cycloolefin polymer is to obtain it through two steps of step (1) polymerization and step (2) hydrogenation. The reaction route is shown as follows:
[0031]
[0032] Specifically, a method for preparing the above-mentioned high barrier cycloolefin polymer comprises the following steps:
[0033] (1) Polymerization:
[0034] S1: subjecting the compound represented by formula Ⅰ-A to ring-opening metathesis polymerization under the action of a catalyst to obtain polymer block I;
[0035] S2: adding the cycloolefin compound represented by formula II-A to the polymer block I prepared in S1 and continuing the polymerization to prepare a diblock copolymer;
[0036] Optional S3: adding a cycloolefin compound represented by formula Ⅰ-A and / or formula Ⅱ-A to the diblock copolymer obtained in step S2 to carry out polymerization reaction to obtain a block copolymer.
[0037] (2) Hydrogenation: The block copolymer obtained in step (1) is subjected to a hydrogenation reaction with hydrogen to obtain the high barrier cycloolefin polymer.
[0038] In the present invention, the polymerization process of step (1) is specifically as follows:
[0039] S1: Add the compound represented by formula Ⅰ-A into a solvent, add a ring-opening metathesis polymerization catalyst to carry out solution polymerization to obtain the polymer block represented by formula Ⅰ. The molar ratio of the compound represented by formula Ⅰ-A to the catalyst is 10-500:1, preferably 10-200:1.
[0040] S2: Add the compound represented by formula II-A to the reaction solution obtained in S1 to carry out solution polymerization reaction to obtain a diblock polymer of formula I-formula II. The molar ratio of the cycloolefin compound represented by formula II-A to the catalyst added in S1 is 50-500:1, preferably 50-200:1.
[0041] Optional S3: When it is necessary to prepare a multi-block copolymer with three or more segments, add Formula Ⅰ-A or Formula Ⅱ-A to the diblock copolymer obtained in step S2 for polymerization reaction, and step S3 can be repeated multiple times as needed to add materials; when it is not necessary to prepare a multi-block copolymer with three or more segments, step (1) is only performed in steps S1 and S2.
[0042] Preferably, each time the feed is added, the molar ratio of the compound represented by formula Ⅰ-A to the catalyst in S1 is 10-500:1, and the molar ratio of the cycloolefin compound represented by formula Ⅱ-A to the catalyst in S1 is 50-500:1.
[0043] Among them, there are many types of ring-opening metathesis polymerization catalysts, and conventional selections in the field can be used. The present invention has no special requirements for them. For example, it can be any one or a combination of at least two of a multi-component tungsten catalyst, a Grubbs series catalyst, and a Schrock series catalyst, preferably a Grubbs series catalyst;
[0044] Wherein, the solvent in step S1 is selected from at least one of aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, halogenated aromatic hydrocarbon solvents, and ether solvents;
[0045] Preferably, the aliphatic hydrocarbon solvent is selected from at least one of n-hexane and heptane;
[0046] Preferably, the alicyclic hydrocarbon solvent is selected from at least one of cyclopentane, cyclohexane, methylcyclohexane and dimethylcyclohexane;
[0047] Preferably, the aromatic hydrocarbon solvent is selected from at least one of benzene, toluene and xylene;
[0048] Preferably, the halogenated aromatic hydrocarbon solvent is selected from at least one of chlorobenzene and dichlorobenzene;
[0049] Preferably, the ether solvent is selected from at least one of diethyl ether and tetrahydrofuran.
[0050] Preferably, the mass of the compound represented by formula Ⅰ-A and the optional cycloolefin compound represented by formula Ⅱ-A accounts for 5 to 70% of the mass of the solvent, such as 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 60, 70%, preferably 20 to 50%;
[0051] Wherein, the solution polymerization reaction has a temperature of 0 to 200°C, such as 0, 10, 30, 50, 80, 100, 130, 150, 180, 200°C, preferably 50 to 150°C; and a time of 1 to 60 min, such as 1, 10, 20, 30, 40, 50, 60 min, preferably 1 to 30 min.
[0052] In the present invention, the hydrogenation process in step (2) is specifically as follows: the block copolymer obtained in step (1) is subjected to a hydrogenation reaction with hydrogen in the presence of a hydrogenation catalyst to obtain the high barrier cycloolefin polymer.
[0053] Wherein, the hydrogenation catalyst includes a homogeneous or heterogeneous catalyst, which can be selected conventionally in the field, and the present invention has no special requirements for it;
[0054] Preferably, the heterogeneous catalyst is selected from at least one of metal-supported silica, metal-supported alumina, metal-supported titanium oxide, skeleton nickel, palladium-carbon catalyst, etc.; wherein the metal is selected from at least one of nickel, palladium, platinum, rhodium, and ruthenium;
[0055] Preferably, the amount of the heterogeneous catalyst added is 0.5-10% of the mass of the reaction solution in step (2), for example 0.5, 1, 3, 5, 7, 9, 10%;
[0056] Preferably, the homogeneous catalyst is selected from at least one of soluble complexes of metals such as nickel, titanium, palladium, platinum, rhodium, ruthenium, etc., such as a Ziegler hydrogenation catalyst composed of nickel salt-alkyl aluminum, a titanocene-alkyl lithium hydrogenation catalyst, a Ru(X)Cl(CO)L2 type complex catalyst, etc.;
[0057] Preferably, the amount of the homogeneous catalyst added is 0.001-10% of the mass of the reaction solution in step (2), such as 0.001, 0.01, 0.1, 0.5, 1, 3, 5, 7, 9, 10%, preferably 2-10% of the mass of the reaction solution;
[0058] The reaction solution in step (2) is the reaction solution obtained in step (1) or the diluted reaction solution.
[0059] Wherein, the hydrogenation reaction is carried out at high temperature and high pressure; the hydrogenation temperature is 80-200°C, for example, 80, 100, 130, 150, 180, 200°C; the amount of hydrogen fed is determined by the charging pressure, and the charging hydrogen pressure is controlled to be the reaction pressure 1-7MPa, for example, 1, 2, 3, 4, 5, 6, 7MPa;
[0060] Preferably, the hydrogenation reaction ends when the molar content of double bonds in the obtained high barrier cycloolefin polymer is ≤50%, such as 50, 45, 40, 35, 30, 25, 20, 15, 10, 5, 1%, preferably ≤1%.
[0061] In the present invention, step (1) also includes terminating the reaction, and step (2) also includes post-treatment processes such as acidification, flocculation, washing, and drying, which are all conventional operations in the art and are not specifically limited in the present invention.
[0062] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0063] The high barrier cycloolefin polymer of the present invention, by introducing strongly electronegative fluorine atoms, enables the cycloolefin polymer of the present invention to form a stronger intermolecular force and form a dense structure to improve the water barrier and oxygen barrier properties of the material; at the same time, the high barrier cycloolefin polymer of the present invention also maintains the excellent optical properties of the cycloolefin polymer. DETAILED DESCRIPTION
[0064] In order to better understand the technical solution of the present invention, the content of the present invention is further described below in conjunction with the following specific embodiments, but the content of the present invention is not limited to the following embodiments.
[0065] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0066] The sources of the raw materials used in the following examples are as follows. Unless otherwise specified, all other raw materials are conventional raw materials in the art, and the purity specifications used are analytically pure or chemically pure:
[0067] High-purity hydrogen: 99.999%, Dalian Guangming Special Gas Co., Ltd.;
[0068] Dicyclopentadiene: 98% (GC), Sigma-Aldrich;
[0069] Norbornene: 98%, TCI;
[0070] Tetracyclododecene: 98%, TCI;
[0071] Trifluoropropylene: 99%, J&K Technology;
[0072] Pentafluorostyrene: 97%, J&K Technologies;
[0073] Trifluorostyrene: 95%, J&K Technologies;
[0074] Grubbs 3rd generation catalyst: 99.95%, Shanghai Aladdin;
[0075] Methyl norbornene: 98%, Shanghai Aladdin;
[0076] Phenylnorbornene: 98%, WuXi AppTec;
[0077] Palladium carbon catalyst: Pd@C, Alfa;
[0078] Nickel acetylacetonate: 95%, Shanghai Aladdin;
[0079] Triisobutylaluminum: 1.0M n-hexane solution, Shanghai Aladdin. The performance test parameters and corresponding test methods used in each embodiment of the present invention are as follows:
[0080] The structures of the compounds and polymers synthesized in the present invention were measured by a Bruker ARX-400 nuclear magnetic resonance spectrometer using deuterated chloroform (CDCl3), deuterated benzene (C6D6), and deuterated 1,1,2,2-tetrachloroethane (C2D2Cl4) as solvents at room temperature or 90°C.
[0081] The molecular weight and molecular weight distribution of the polymer synthesized in the present invention were obtained by testing at 150° C. using PL-GPC220, using three PLgel 10 μm MIXED-B separation columns connected in series and 1,2,4-trichlorobenzene as the solvent;
[0082] The water vapor permeability of polymers is measured according to GB / T1037 standard;
[0083] The oxygen permeability of polymers is measured according to GB / T1038 standard;
[0084] The visible light transmittance of the polymer is measured according to GB / T2410 standard. Specific embodiments
[0086] (I) Monomer preparation
[0087] Monomer Synthesis Example-1
[0088]
[0089] In a 2L stainless steel autoclave, add 3.8 mol of dicyclopentadiene, 9.6 mol of trifluoropropylene, and 0.06 mol of 2,6-di-tert-butyl-4-methylphenol. After replacing the atmosphere in the autoclave with nitrogen, heat to 180°C, start stirring, and react for 6 hours. After the reaction is completed, cool the autoclave to room temperature, and purify the reactant by column chromatography (ethyl acetate / petroleum ether=1 / 13) to obtain the corresponding monomer. 1H NMR (400MHz, CDCl3): δ=6.16(1H), δ=5.96(1H), δ=2.95–2.89(2H), δ=2.66(1H); δ=2.06(1H); δ=1.49-1.59(2H); δ=1.13(1H).
[0090] Monomer Synthesis Example-2
[0091]
[0092] The preparation of monomer M-2 is the same as that of monomer M-1, except that trifluorostyrene is used instead of trifluoropropylene. 1HNMR (400MHz, CDCl3): δ=7.08(2H), δ=6.24(1H), δ=5.88(1H), δ=2.93–3.05(3H); δ=2.00(1H); δ=1.47-1.58(2H); δ=1.09(1H).
[0093] Monomer Synthesis Example-3
[0094]
[0095] The preparation of monomer M-3 is the same as that of monomer M-1, except that pentafluorostyrene is used instead of trifluoropropylene. 1HNMR (400MHz, CDCl3): δ=6.24(1H), δ=5.87(m,1H), δ=3.56(1H), δ=3.13(1H); δ=2.94(1H); δ=2.10(1H); δ=1.47-1.58(2H); δ=1.19(1H).
[0096] Monomer Synthesis Example-4
[0097]
[0098] The preparation of monomer M-4 is the same as that of monomer M-1, except that trifluoropropylene is replaced by M-2. 1H NMR (400MHz, CDCl3): δ=7.09 (2H), δ=5.85 (2H), δ=2.93–3.05 (3H); δ=3.42 (1H); δ=2.85-2.87 (2H); δ=2.12 (1H); δ=1.93-1.99 (2H); δ=1.72 (1H); δ=1.56 (1H); δ=1.45 (1H); δ=1.34 (2H); δ=1.21 (1H); δ=1.04 (1H).
[0099] Monomer Synthesis Example-5
[0100]
[0101] In a 2L stainless steel autoclave, 1.9 mol of dicyclopentadiene, 4.1 mol of monomer M-1, and 0.03 mol of 2,6-di-tert-butyl-4-methylphenol were added, and the atmosphere in the autoclave was replaced with nitrogen, and then heated to 180°C and stirred. After reacting for 6 hours, the autoclave was cooled to room temperature, and 1.8 mol of dicyclopentadiene was added to the autoclave. After the atmosphere in the autoclave was replaced with nitrogen again, it was heated to 160°C, stirred, and reacted for 8 hours. After the reaction was completed, the reactant was purified by column chromatography (ethyl acetate / petroleum ether=1 / 16) to obtain the corresponding monomer. 1H NMR (400MHz, CDCl3): δ=5.85 (2H), δ=2.88–2.82 (3H); δ=2.10-1.95 (6H); δ=1.84-1.56 (6H); δ=1.35-1.31 (3H); δ=1.04 (1H).
[0102] (II) Polymer preparation
[0103] Example 1
[0104] HPM-1 preparation
[0105]
[0106] (1-1) Preparation of Ring-Opening Polymer (PM-1)
[0107] In the glove box, take 1.6g (10mmol) of monomer M-1, dissolve it in 20g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.8g (1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 13.2g (100mmol) of dicyclopentadiene, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 1.6g (10mmol) of M-1, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 60g. The weight average molecular weight Mw of the ring-opening polymer is 2.5×10 4 , the conversion rate of monomer to polymer is >99%.
[0108] (1-2) Preparation of Cycloolefin Polymer (HPM-1) by Hydrogenation of Ring-Opening Polymer
[0109] In a glove box, 51.6 mg (200 μmol) of nickel acetylacetonate was weighed and dispersed in 5 g of xylene. 0.8 g (1.0 mmol) of triisobutylaluminum was extracted and injected into the nickel acetylacetonate. The mixture was reacted for 2 min to prepare a hydrogenation catalyst.
[0110] Weigh 60g of the ring-opening polymer reaction liquid in (1-1), add 30g of xylene to dilute it, and transfer it to a stainless steel reactor that has been dried in advance, and replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Inject 5g of the above-prepared hydrogenation catalyst into the reactor, pressurize it to 4MPa with hydrogen, start stirring and heat to 80°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction, and the corresponding hydrogenated polymer solution is obtained. After cooling, the reaction solution is poured into acidified ethanol, flocculated and washed three times, and the precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, namely polymer HPM-1, has a weight-average molecular weight Mw of 2.7×10 4 , the residual double bonds are less than 1%.
[0111] (1-3) Preparation of hydrogenated polymer membrane
[0112] Take 5 g of the polymer obtained in step (1-2) and add 20 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding polymer film.
[0113] The transmittance, water vapor permeability, oxygen permeability, etc. of the polymer HPM-1 obtained by the above-mentioned method are shown in Table 1.
[0114] Example 2
[0115] HPM-2 preparation
[0116]
[0117] (2-1) Preparation of Ring-Opening Polymer (PM-2)
[0118] In the glove box, take 4.5g (20mmol) of monomer M-2, dissolve it in 30g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.8g (1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 4.6g (35mmol) of dicyclopentadiene and 1.4g (15mmol) of norbornene, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 4.5g (20mmol) of M-2, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 70g. The weight average molecular weight Mw of the ring-opening polymer is 2.8×10 4 , the conversion rate of monomer to polymer is >99%.
[0119] (2-2) Hydrogenation of Ring-Opening Polymer (HPM-2)
[0120] Weigh 60g of the ring-opening polymer reaction liquid in (2-1), add 10g of cyclohexane to dilute it, and transfer it to a stainless steel reactor that has been dried in advance. Add 2.8g of palladium carbon catalyst to the reactor. After sealing the reactor, replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Pressurize it to 4MPa with hydrogen, start stirring and heat to 130°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction. The corresponding hydrogenated polymer solution is obtained. After cooling, centrifugation is performed, and the supernatant is poured into acidified ethanol. Flocculation and washing are performed three times. The precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, i.e., polymer HPM-2, has a weight-average molecular weight Mw of 2.9×10 4 , the residual double bonds are less than 1%.
[0121] (2-3) Preparation of hydrogenated polymer membrane
[0122] Take 5 g of the hydrogenated polymer obtained in step (2-2) and add 10 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding hydrogenated polymer film.
[0123] The permeability, water vapor permeability, oxygen permeability, etc. of the polymer HPM-2 obtained by the aforementioned method are tested and the results are shown in Table 1.
[0124] Example 3
[0125] HPM-3 preparation
[0126]
[0127] (3-1) Preparation of Ring-Opening Polymer (PM-3)
[0128] In the glove box, take 5.8g (20mmol) of monomer M-4, dissolve it in 30g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.8g (1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 3.33g (25mmol) of dicyclopentadiene and 4.0g (25mmol) of tetracyclododecene, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 6.8g (20mmol) of M-4, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 70g. The weight average molecular weight Mw of the ring-opening polymer is 3.1×10 4 , the conversion rate of monomer to polymer is >99%.
[0129] (3-2) Hydrogenation of Ring-Opening Polymer (HPM-3)
[0130] In a glove box, 25.8 mg (100 μmol) of nickel acetylacetonate was weighed and dispersed in 5 g of xylene. 0.4 g (0.5 mmol) of triisobutylaluminum was extracted and injected into the nickel acetylacetonate. The mixture was reacted for 2 min to prepare a hydrogenation catalyst.
[0131] Weigh 30g of the ring-opening polymer reaction liquid in (3-1), add 10g of xylene to dilute it, and transfer it to a stainless steel reactor that has been dried in advance, and replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Inject 1g of the hydrogenation catalyst prepared above into the reactor, pressurize it to 4MPa with hydrogen, start stirring and heat to 80°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction, and the corresponding hydrogenated polymer solution is obtained. After cooling, the reaction solution is poured into acidified ethanol, flocculated and washed three times, and the precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, namely polymer HPM-3, has a weight average molecular weight Mw of 3.3×10 4 , the residual double bonds are less than 1%.
[0132] (3-3) Preparation of hydrogenated polymer membrane
[0133] Take 5 g of the hydrogenated polymer obtained in step (3-2) and add 10 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding hydrogenated polymer film.
[0134] The transmittance, water vapor permeability, oxygen permeability, etc. of the polymer HPM-3 obtained by testing the above method are shown in Table 1.
[0135] Example 4
[0136] HPM-4 Preparation
[0137]
[0138] (4-1) Preparation of Ring-Opening Polymer (PM-4)
[0139] In the glove box, take 3.9g (15mmol) of monomer M-3, dissolve it in 30g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.8g (1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 13.2g (100mmol) of dicyclopentadiene, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 3.9g (15mmol) of M-3, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 70g. The weight average molecular weight Mw of the ring-opening polymer is 4.1×10 4 , the conversion rate of monomer to polymer is >99%.
[0140] (4-2) Hydrogenation of Ring-Opening Polymer (HPM-4)
[0141] In a glove box, 25.8 μmol (100 μmol) of nickel acetylacetonate was weighed and dispersed in 5 g of xylene. 0.4 g (0.5 mmol) of triisobutylaluminum was extracted and injected into the nickel acetylacetonate. The mixture was reacted for 2 min to prepare a hydrogenation catalyst.
[0142] Weigh 20g of the ring-opening polymer reaction liquid in (4-1), add 20g of xylene to dilute it, and transfer it to a stainless steel reactor that has been dried in advance, and replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Inject 2g of the hydrogenation catalyst prepared above into the reactor, pressurize it to 4MPa with hydrogen, start stirring and heat to 80°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction, and the corresponding hydrogenated polymer solution is obtained. After cooling, the reaction solution is poured into acidified ethanol, flocculated and washed three times, and the precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, namely polymer HPM-4, has a weight-average molecular weight Mw of 4.5×10 4 , the residual double bonds are less than 1%.
[0143] (4-3) Preparation of hydrogenated polymer membrane
[0144] Take 5 g of the hydrogenated polymer obtained in step (4-2) and add 10 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding hydrogenated polymer film.
[0145] The transmittance, water vapor permeability, oxygen permeability, etc. of the polymer HPM-4 obtained by the aforementioned method are tested and the results are shown in Table 1.
[0146] Example 5
[0147] HPM-1-2 preparation
[0148] (5-1) Preparation of Ring-Opening Polymer (PM-1-2)
[0149] In the glove box, take 8.1g (50mmol) of monomer M-1, dissolve it in 30g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.08g (0.1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 5.9g (50mmol) of dicyclopentadiene, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 8.1g (50mmol) of M-1, dissolve it in 30g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 80g. The weight average molecular weight Mw of the ring-opening polymer is 24.5×10 4, the conversion rate of monomer to polymer is >99%.
[0150] (5-2) Hydrogenation of Ring-Opening Polymer (HPM-1-2)
[0151] In a glove box, 25.8 μmol (100 μmol) of nickel acetylacetonate was weighed and dispersed in 5 g of decahydronaphthalene. 0.4 g (0.5 mmol) of triisobutylaluminum was extracted and injected into the nickel acetylacetonate. The mixture was reacted for 2 min to prepare a hydrogenation catalyst.
[0152] Weigh 20g of the ring-opening polymer reaction liquid in (5-1), add 20g of xylene to dilute it, and transfer it to a stainless steel reactor that has been dried in advance, and replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Inject 2g of the hydrogenation catalyst prepared above into the reactor, pressurize it to 4MPa with hydrogen, start stirring and heat to 80°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction, and the corresponding hydrogenated polymer solution is obtained. After cooling, the reaction solution is poured into acidified ethanol, flocculated and washed three times, and the precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, namely polymer HPM-1-2, has a weight-average molecular weight Mw of 25.5×10 4 , the residual double bonds are less than 1%.
[0153] (5-3) Preparation of hydrogenated polymer membrane
[0154] Take 5 g of the hydrogenated polymer obtained in step (5-2) and add 10 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding hydrogenated polymer film.
[0155] The transmittance, water vapor permeability, oxygen permeability, etc. of the polymer HPM-1-2 were tested by the aforementioned method, and the results are shown in Table 1.
[0156] Example 6
[0157] HPM-5 preparation
[0158]
[0159] (6-1) Preparation of Ring-Opening Polymer (PM-5)
[0160] In the glove box, take 16.8g (75mmol) of monomer M-2, dissolve it in 40g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.8g (1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 6.6g (50mmol) of dicyclopentadiene and 8.0g (50mmol) of tetracyclododecene, dissolve it in 40g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 16.8g (75mmol) of M-2, dissolve it in 40g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 120g. The weight average molecular weight Mw of the ring-opening polymer is 4.9×10 4 , the conversion rate of monomer to polymer is >99%.
[0161] (6-2) Hydrogenation of Ring-Opening Polymer (HPM-5)
[0162] In a glove box, 25.8 μmol (100 μmol) of nickel acetylacetonate was weighed and dispersed in 5 g of decahydronaphthalene. 0.4 g (0.5 mmol) of triisobutylaluminum was extracted and injected into the nickel acetylacetonate. The mixture was reacted for 2 min to prepare a hydrogenation catalyst.
[0163] Weigh 20g of the ring-opening polymer reaction liquid in (6-1), add 20g of xylene to dilute it, and transfer it to a stainless steel reactor that has been dried in advance, and replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Inject 2g of the hydrogenation catalyst prepared above into the reactor, pressurize it to 4MPa with hydrogen, start stirring and heat to 80°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction, and the corresponding hydrogenated polymer solution is obtained. After cooling, the reaction solution is poured into acidified ethanol, flocculated and washed three times, and the precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, namely polymer HPM-5, has a weight-average molecular weight Mw of 5.2×10 4 , the residual double bonds are less than 1%.
[0164] (6-3) Preparation of hydrogenated polymer membrane
[0165] Take 5 g of the hydrogenated polymer obtained in step (6-2) and add 10 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding hydrogenated polymer film.
[0166] The transmittance, water vapor permeability, oxygen permeability, etc. of the polymer HPM-5 obtained by the aforementioned method are tested and the results are shown in Table 1.
[0167] Example 7
[0168] HPM-6 Preparation
[0169]
[0170] (7-1) Preparation of Ring-Opening Polymer (PM-6)
[0171] In the glove box, take 1.6g (10mmol) of monomer M-1, dissolve it in 20g of xylene and add it to a 250ml flask equipped with a magnet, start stirring and heating; when the temperature rises to 40°C, add 0.8g (1mmol) of Grubbs third-generation catalyst to the flask to start polymerization. After 30 minutes of polymerization, take 13.2g (100mmol) of dicyclopentadiene, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction; after 30 minutes of polymerization, take 2.9g (10mmol) of M-5, dissolve it in 20g of xylene and add it to the reaction solution to continue the reaction for 30 minutes; add 1g of ethanol to terminate the active center. The total amount of the reaction solution is 78g. The weight average molecular weight Mw of the ring-opening polymer is 3.6×10 4 , the conversion rate of monomer to polymer is >99%.
[0172] (7-2) Preparation of Cycloolefin Polymer (HPM-6) by Hydrogenation of Ring-Opening Polymer
[0173] In a glove box, 51.6 mg (200 μmol) of nickel acetylacetonate was weighed and dispersed in 5 g of xylene. 0.8 g (1.0 mmol) of triisobutylaluminum was extracted and injected into the nickel acetylacetonate. The mixture was reacted for 2 min to prepare a hydrogenation catalyst.
[0174] Weigh 60g of the ring-opening polymer reaction liquid in (1-1), add 30g of xylene to dilute it, and transfer it to a stainless steel reactor that has been dried in advance, and replace the atmosphere in the reactor with nitrogen and hydrogen three times in sequence. Inject 5g of the above-prepared hydrogenation catalyst into the reactor, pressurize it to 4MPa with hydrogen, start stirring and heat to 80°C. After 4 hours of reaction, the double bond content in the product is reduced to 1%, which is the end point of the hydrogenation reaction, and the corresponding hydrogenated polymer solution is obtained. After cooling, the reaction solution is poured into acidified ethanol, flocculated and washed three times, and the precipitated polymer is washed three times with deionized water and dried in a vacuum oven. The obtained hydrogenated polymer, namely polymer HPM-6, has a weight-average molecular weight Mw of 2.7×10 4 , the residual double bonds are less than 1%.
[0175] (7-3) Preparation of hydrogenated polymer membrane
[0176] Take 5 g of the polymer obtained in step (7-2) and add 20 ml of xylene to dissolve it. Pour the dissolved polymer solution into a clean mold and evaporate the solvent to obtain the corresponding polymer film.
[0177] The transmittance, water vapor permeability, oxygen permeability, etc. of the polymer HPM-6 obtained by the aforementioned method are tested and the results are shown in Table 1.
[0178] Comparative Example 1
[0179] The preparation method was prepared by referring to Example 1, except that the monomer M-1 was replaced by an equal amount of methyl norbornene, and other operations and parameters remained unchanged to obtain a polymer. The performance test results are shown in Table 1.
[0180] Comparative Example 2
[0181] The preparation method was referred to Example 2, except that the monomer M-2 was replaced by an equal amount of phenyl norbornene, and other operations and parameters remained unchanged to obtain a polymer. The performance test results are shown in Table 1.
[0182] In addition, the performance of three brands of cycloolefin polymers, namely, ZEONEX K26R and ZEONEX 690R of ZEON Company and ARTON F4520 of JSR Company, which are the mainstream commercial products on the market, were also measured under the same conditions. The results are shown in Table 1.
[0183] Table 1 Physical properties of polymers prepared in the examples of the present invention and comparative examples and properties of commercially available cycloolefin polymers
[0184]
[0185] Compared with the mainstream commercial cycloolefin polymer grades and comparative examples, the water vapor permeation rate and oxygen permeation rate are significantly reduced, while the material has high transparency. According to the present invention, a barrier material that is advantageously used as packaging can be provided.
Claims
1. A high barrier cycloolefin polymer, characterized in that: Contains the structural unit shown in the following formula I: In formula I, L is -CH2-CH2- or -CH=CH-; n is an integer from 0 to 2; R is a fluoroalkyl group or a fluoroaryl group, preferably one or more of trifluoromethyl, pentafluoroethyl, heptafluoropropyl, trifluorophenyl and pentafluorophenyl; and x is 10-500.
2. The high barrier cycloolefin polymer according to claim 1, characterized in that: Contains the structural unit shown in the following formula II: In Formula II, RC is any one of an alkyl group and a cycloalkyl group, preferably a C4-C8 alkyl group, a C5-C 15 Any of the cycloalkyl groups of C4-C8, more preferably C4-C8 alkylene groups, C5-C 15 Any one of the groups containing a cyclopentane structure; y is 50-500.
3. The high barrier cycloolefin polymer according to any one of claims 1 to 2, characterized in that: The total number of blocks of the structural units represented by formula I and formula II is 2-5.
4. The high barrier cycloolefin polymer according to claim 1, characterized in that: The structural unit shown in formula I is prepared from the compound shown in formula I-A: In formula Ⅰ-A, R and n are defined the same as R and n in the above formula Ⅰ; Preferably, the compound represented by formula Ⅰ-A is selected from at least one of compounds M-1, M-2, M-3, M-4, and M-5 having the following structures:
5. The high barrier cycloolefin polymer according to claim 2, characterized in that: The structural unit shown in formula II is prepared by the cycloolefin compound shown in formula II-A: Wherein, the definition of RC is the same as that of RC in Formula II; Preferably, the cycloolefin compound represented by formula II-A is at least one selected from cyclopentene, cyclohexene, cycloheptene, cyclooctene, cyclooctadiene, norbornene, dicyclopentadiene and tetracyclododecene.
6. The high barrier cycloolefin polymer according to any one of claims 1 to 5, characterized in that: The high barrier cycloolefin polymer has a number average molecular weight of 5000-100000; and / or the high barrier cycloolefin polymer has a double bond molar content of ≤50%, preferably ≤1%.
7. A method for preparing a high barrier cycloolefin polymer according to any one of claims 1 to 6, characterized in that the steps include: (1) Polymerization: S1: subjecting the compound represented by formula Ⅰ-A to ring-opening metathesis polymerization under the action of a catalyst to obtain polymer block I; S2: adding the cycloolefin compound represented by formula II-A to the polymer block I prepared in S1 and continuing the polymerization to prepare a diblock copolymer; Optional S3: adding a cycloolefin compound represented by formula Ⅰ-A and / or formula Ⅱ-A to the diblock copolymer obtained in step S2 to carry out polymerization reaction to obtain a multiblock copolymer; (2) Hydrogenation: The block copolymer obtained by polymerization in step (1) is subjected to a hydrogenation reaction with hydrogen to obtain a high barrier cycloolefin polymer.
8. The preparation method according to claim 7, characterized in that: A certain proportion of the compound represented by formula Ⅰ-A and the cycloolefin compound represented by formula Ⅱ-A are added to a solvent, and a ring-opening metathesis polymerization catalyst is added to carry out a polymerization reaction; Preferably, the ring-opening metathesis polymerization catalyst is any one of a multi-component tungsten series catalyst, a Grubbs series catalyst, and a Schrock series catalyst, or a combination of at least two of them, preferably a Grubbs series catalyst; Preferably, the solvent is selected from at least one of aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, halogenated aromatic hydrocarbon solvents, and ether solvents; Preferably, the aliphatic hydrocarbon solvent is selected from at least one of n-hexane and heptane; Preferably, the alicyclic hydrocarbon solvent is selected from at least one of cyclopentane, cyclohexane, methylcyclohexane and dimethylcyclohexane; Preferably, the aromatic hydrocarbon solvent is selected from at least one of benzene, toluene and xylene; Preferably, the halogenated aromatic hydrocarbon solvent is selected from at least one of chlorobenzene and dichlorobenzene; Preferably, the ether solvent is selected from at least one of diethyl ether and tetrahydrofuran; Preferably, the mass of the compound represented by formula Ⅰ-A and the cycloolefin compound represented by formula Ⅱ-A accounts for 5 to 70% of the mass of the solvent, preferably 20 to 50%; Preferably, the mass ratio of the compound represented by formula Ⅰ-A added each time in the optional step S3 to the ring-opening metathesis polymerization catalyst is 10 to 500:1; Preferably, the mass ratio of the cycloolefin compound represented by formula II-A to the ring-opening metathesis polymerization catalyst added each time in the optional step S3 is 50 to 500:1; The polymerization reaction temperature is 0 to 200° C., preferably 50 to 150° C.; the polymerization reaction time is 1 to 60 minutes, preferably 5 to 30 minutes.
9. The preparation method according to claim 7 or 8, characterized in that: The step (2) hydrogenation specifically comprises: subjecting the block copolymer obtained in the step (1) to a hydrogenation reaction with hydrogen in the presence of a hydrogenation catalyst to obtain a high barrier cycloolefin polymer; Preferably, the hydrogenation catalyst comprises a homogeneous or heterogeneous catalyst, More preferably, the heterogeneous catalyst is selected from at least one of metal-supported silica, metal-supported alumina, metal-supported titanium oxide, skeleton nickel, and palladium-carbon catalyst; wherein the metal is selected from at least one of nickel, palladium, platinum, rhodium, and ruthenium; preferably, the amount of the heterogeneous catalyst added is 0.5 to 10% of the mass of the reaction solution in step (2); More preferably, the homogeneous catalyst is selected from at least one of soluble complexes of nickel, titanium, palladium, platinum, rhodium and ruthenium metals; preferably, the amount of the homogeneous catalyst added is 0.001 to 10% of the mass of the reaction solution in step (2).
10. The preparation method according to claim 9, characterized in that: The temperature of the hydrogenation reaction in step (2) is 80-200° C.; the amount of hydrogen fed is determined by the charging pressure, and the charging pressure of hydrogen is controlled to be 1-7 MPa; Preferably, the hydrogenation reaction ends when the molar content of double bonds in the obtained high barrier cycloolefin polymer is ≤50%, more preferably ≤1%.
Citation Information
Patent Citations
Cycloolefin copolymer as well as preparation method and application thereof
CN110669207A
Optical material
CN117624555A
Phenylfluorene type cycloolefin polymer and preparation method thereof
CN117801228A
Optical part using fluorine-containing cyclic olefin polymer
JP2007177046A
Method of producing cyclic olefin ring-opened polymer
JP2015178561A