PBET copolyester and preparation method thereof

CN118930822APending Publication Date: 2024-11-12NAT POLYMER MATERIALS IND INNOVATION CENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310526955.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

[0009]本发明的目的在于,克服现有技术中重金属含量高、力学性能差的缺陷,提供一种PBET共聚酯

Benefits of technology

[0070] The present invention develops a PBET copolyester and its preparation method. The PBET copolyester of the present invention uses waste polyester as raw material, and through the steps of initial depolymerization, re-depolymerization and polycondensation, a PBET copolyester with low heavy metal content and suitable crystallinity is produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930822A_ABST
    Figure CN118930822A_ABST
Patent Text Reader

Abstract

The invention provides PBET copolyester and a preparation method thereof, and belongs to the technical field of recycled polyester. The PBET copolyester disclosed by the invention is derived to a repeating unit of the following components: a component A: aromatic dicarboxylic acid; based on the total molar weight of the component B, the component B comprises 60-96 mol% of 1, 4-butanediol or 1, 3-butanediol and 4-40 mol% of ethylene glycol; the crystallinity of the PBET copolyester is 5-20%, the zinc content in the PBET copolyester is less than or equal to 100 ppm, and the titanium content in the PBET copolyester is less than or equal to 120 ppm. According to the present invention, the PBET copolyester is adopted as the PBET copolyester, and the waste polyester is adopted as the raw material to prepare the PBET copolyester with characteristics of low heavy metal content and suitable crystallinity through the steps of primary depolymerization, secondary depolymerization and polycondensation;
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of recycled polyester, in particular to a PBET copolyester and a preparation method thereof. Background Art

[0002] At present, degradable plastics account for about 58% of plastic production worldwide, and non-degradable plastics account for 42%. The treatment of waste plastics is an urgent problem to be solved. In the future, my country will gradually solve the harm caused by traditional waste plastic treatment to the environment through source reduction, reuse, use of bio-based or biodegradable plastics instead of fossil-based materials, and plastic recycling through physical or chemical recycling.

[0003] Polyesters such as PBT and PET are the main raw materials for plastics. Since PET contains carbonyl groups on its main chain, from the perspective of thermodynamics and kinetics, PET is a product with recycling value and easy to achieve industrial recycling. It has strong recyclability and is easier to physically and chemically depolymerize than other plastics. At present, the main methods for recycling PET are physical recycling and chemical recycling. Among them, the main methods for chemical recycling are alcoholysis, hydrolysis, aminolysis, glycolysis, and chemical combination.

[0004] There is an existing technology (Zhou Nan, Song Chenxing. Research and development of PBET copolyester [J]. Chemical Technology Market, 2001, 24 (8): 3.) that uses dimethyl terephthalate (DMT), 1,4-butanediol (1,4-BG), and ethylene glycol (EG) as raw materials, and polycondenses to prepare a terpolymer: PBET copolyester, which has the advantages of PBT and PET. However, in this preparation method, three fossil-based raw materials are used instead of waste polyester as raw materials, and the preparation requires special processes and reactors.

[0005] Chinese patent application CN114031756A discloses a closed-loop method for recycling waste polyester to prepare recycled polyester with typical green and low-carbon characteristics, which includes depolymerizing waste polyester under microwave conditions; removing the polyol solvent from the depolymerization product, purifying and removing byproducts to obtain a depolymerized monomer; mixing the depolymerized monomer with a dibasic acid, a polyol, a polymerization catalyst and a chain extender, and performing an esterification reaction and a polycondensation reaction to obtain a recycled polyester. Although the prior art provides a method for preparing recycled polyester using waste polyester as a raw material, in this method, ethylene glycol must be separated after alcoholysis, and the monomer must be purified, which is not only a cumbersome process, but also causes some reinforcing additives in the waste polyester to be removed during the purification process, resulting in poor mechanical properties of the obtained recycled polyester.

[0006] There is also an existing technology (Zhang Hongming, Zhao Junyu, Gao Fengxiang, et al. Research on the depolymerization-cocondensation "one-pot" synthesis of biodegradable polymers of PET [J]. Journal of Polymer Science, 2022(009):053.) that uses diols of different structures to hydrolyze PET into low molecular weight prepolymers, and then adds dibasic acids for further esterification and polycondensation, so that the depolymerization and copolymerization of PET are completed by the "one-pot method", eliminating the monomer purification process. Although this method uses the one-pot method to eliminate the purification process, since the recycled materials usually contain different amounts of heavy metals, and heavy metal catalysts are also used in the depolymerization process, the catalyst residue will seriously affect the physical properties and aging resistance of the product.

[0007] Currently, PBT materials used in engineering plastics are also widely used in toys and precision instruments, which require good dimensional stability. Therefore, as PCR is used more and more widely, ABS and recycled PBT or recycled PET are generally used in toys to increase the content of PCR. However, the dimensional stability of PBT and PET is slightly poor.

[0008] Therefore, it is necessary to provide a recycled PBET copolyester that meets the requirements of low residual heavy metal content, good mechanical properties, good dimensional stability and low mold shrinkage, meets the requirements of toys and precision instruments for dimensional stability, and can replace some of the application areas of PBT and PET. Summary of the invention

[0009] The purpose of the present invention is to overcome the defects of high heavy metal content and poor mechanical properties in the prior art and to provide a PBET copolyester.

[0010] Another object of the present invention is to provide a method for preparing the above-mentioned PBET copolyester.

[0011] To achieve the above object, the present invention adopts the following technical solution:

[0012] A PBET copolyester derived from repeating units of:

[0013] Component A: aromatic dicarboxylic acid;

[0014] Component B: based on the total molar amount of component B, comprising 60 to 96 mol% of 1,4-butanediol or 1,3-butanediol and 4 to 40 mol% of ethylene glycol;

[0015] The crystallinity of the PBET copolyester is 5-20%, including but not limited to 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%;

[0016] The zinc content in the PBET copolyester is ≤100 ppm, and the titanium content is ≤120 ppm.

[0017] The PBET copolyester of the present invention is a recycled PBET copolyester, comprising a dicarboxylic acid component with aromatic dicarboxylic acid as a repeating unit and a diol component with butanediol and ethylene glycol as repeating units, and the PBET copolyester has an extremely low heavy metal content, wherein the zinc content is ≤100ppm and the titanium content is ≤120ppm. The zinc and titanium residues in the PBET copolyester are introduced by the catalyst used in the depolymerization and polycondensation processes on the one hand, and are also introduced by impurities in the waste polyester raw materials on the other hand.

[0018] The crystallinity of recycled polyester is one of the main parameters of standard polymer properties and an important indicator for measuring its quality. The PBET copolyester of the present invention has a low crystallinity of 5-20%. The PBET copolyester has good mechanical properties, especially excellent impact resistance; at the same time, within the above-mentioned suitable crystallinity range, the PBET copolyester also has good dimensional stability and low mold shrinkage, so it can be applied to the field of toys and precision instrument modified materials.

[0019] Preferably, the zinc content in the PBET copolyester is 25 to 70 ppm, and the titanium content is 40 to 85 ppm.

[0020] Preferably, the calcium content in the PBET copolyester is ≤50 ppm.

[0021] More preferably, the calcium content in the PBET copolyester is 15 to 35 ppm.

[0022] In the present invention, the crystallinity of the PBET copolyester is analyzed using an X-ray diffractometer (XRD) with reference to standard JY / T0587-2020. Specifically, a D8 ADVANCE X-ray diffractometer from BRUKER, Germany, is used, at room temperature, CuKa rays (λ=0.154 nm), collected once every 0.05°, and the scanning angle range is 6° to 60°.

[0023] In the present invention, the zinc content and the titanium content are tested according to the following method:

[0024] Inductively coupled plasma atomic emission spectrometer ICP-OES was used according to the standard inductively coupled plasma atomic emission spectrometer determination method US EPA 6010C:2014.

[0025] Preferably, the melting point of the PBET copolyester is 200-220°C, including but not limited to 200°C, 201°C, 202°C, 203°C, 204°C, 205°C, 206°C, 207°C, 208°C, 209°C, 210°C, 211°C, 212°C, 213°C, 214°C, 215°C, 216°C, 217°C, 218°C, 219°C, and 220°C.

[0026] The melting point was tested using a differential scanning calorimeter according to ISO 11357-3:2018.

[0027] Preferably, the relative viscosity of the PBET copolyester is 1.4 to 1.8.

[0028] The relative viscosity is tested as follows:

[0029] According to the GB / T 17931-1999 standard method, the sample concentration was 5 mg / ml in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05°C.

[0030] Preferably, the terminal carboxyl content of the PBET copolyester is 20 to 37 mmol / t, including but not limited to 20 mmol / t, 21 mmol / t, 22 mmol / t, 23 mmol / t, 24 mmol / t, 25 mmol / t, 26 mmol / t, 27 mmol / t, 28 mmol / t, 29 mmol / t, 30 mmol / t, 31 mmol / t, 32 mmol / t, 33 mmol / t, 34 mmol / t, 35 mmol / t, 36 mmol / t, and 37 mmol / t.

[0031] The terminal carboxyl content is tested according to standard FZ / T 50012-2006 using automatic potentiometric titration analysis.

[0032] The present invention also protects a method for preparing the above-mentioned PBET copolyester, comprising the following steps:

[0033] S1. Initial depolymerization:

[0034] Dissolving the waste polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product;

[0035] The waste polyester includes one or more of recycled polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and PET / PBT alloy;

[0036] The temperature of the initial depolymerization reaction is 180-230°C and the time is 20-120 minutes;

[0037] S2. Re-depolymerization:

[0038] Extracting part of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions, and filtering the reactant to obtain a filtrate as the re-depolymerization product;

[0039] The temperature of the re-depolymerization reaction is 160-190°C and the time is 10-20 minutes;

[0040] S3. Polycondensation:

[0041] After removing excess alcohol from the re-depolymerization product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, and a polycondensation reaction is carried out under vacuum conditions to obtain the PBET copolyester.

[0042] The preparation method of the PBET copolyester of the present invention uses waste polyester as a raw material, and obtains the PBET copolyester with low heavy metal content, suitable crystallinity and excellent dimensional stability through two steps of alcoholysis and polycondensation, and by controlling factors such as the temperature and time of depolymerization and re-depolymerization.

[0043] In the initial depolymerization step, the waste polyester is subjected to preliminary alcoholysis in the presence of a depolymerization catalyst under normal pressure, inert gas atmosphere, and microwave conditions. The temperature of the initial depolymerization reaction is relatively high, and most of the waste polyester is alcoholyzed into monomers or oligomers. Then, part of the ethylene glycol is extracted from the product of the initial depolymerization, and after adding a chelating agent, a second alcoholysis, i.e., re-depolymerization, is performed. The temperature of the re-depolymerization is lower than that of the initial depolymerization, and the time is shorter. Under the action of the chelating agent, most of the heavy metal ions in the waste polyester are removed synchronously during the re-depolymerization process, and the addition of the chelating agent will not have a negative impact on the mechanical properties, dimensional stability, or crystallinity of the recycled polyester.

[0044] In the preparation method of the present invention, part of the diol is extracted in step S2, and the diol is a byproduct of the initial depolymerization, and the excess alcohol is removed in step S3, both of which are for obtaining a PBET copolyester with an appropriate monomer content. The PBET copolyester finally obtained meets the following characteristics: the PBET copolyester is derived from repeating units of the following components: component A: aromatic dicarboxylic acid; component B: based on the total molar amount of component B, including 60 to 96 mol% of 1,4-butanediol or 1,3-butanediol and 4 to 40% mol% of ethylene glycol;

[0045] In step S2, the method for extracting part of the diol can be vacuum distillation, and the extraction time is 15-60 minutes.

[0046] Optionally, sources of the waste polyester include but are not limited to post-consumer recycled plastics (Post Consumer Recycled Plastic, PCR), industrial recycled plastics (Post Industry Recycle Plastic, PIR), ocean bound plastics (Ocean Bound Plastic, OBP), and in the ocean plastics (IOP).

[0047] Preferably, the waste polyester further includes the steps of impurity removal, cleaning and crushing before the initial depolymerization.

[0048] Preferably, in step S2, the chelating agent is a biomass chelating agent.

[0049] Preferably, the chelating agent includes at least one of chitosan, activated carbon, lignin and phytic acid.

[0050] More preferably, the chelating agent is phytic acid.

[0051] Phytic acid as a chelating agent can not only efficiently chelate the residual metal ions in waste polyester, but also is an excellent antioxidant and stabilizer for recycled PET and PBT. The inventors found that using phytic acid as a chelating agent can obtain PBET copolyester with lower metal ion content, relatively better toughness and better dimensional stability.

[0052] Preferably, in step S2, the amount of the chelating agent added is 0.01-0.1 wt.% of the waste polyester.

[0053] The chelating agent can be added in a relatively low amount to effectively remove metal ions from waste polyester.

[0054] Preferably, in step S1, the depolymerization catalyst includes at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate.

[0055] Preferably, in step S1, the amount of the depolymerization catalyst added is 0.05-0.5 wt.% of the waste polyester.

[0056] Preferably, when the waste polyester contains PET, the alcohol solvent contains 1,4-butanediol; when the waste polyester contains PBT, the alcohol solvent contains ethylene glycol.

[0057] Preferably, the mass ratio of the waste polyester to the alcohol solvent is 1:0.5 to 1:2.

[0058] The alcohol solvent plays the role of alcoholysis, and the inventors have found that 1.4-butanediol has a good alcoholysis effect on the recycled PBT and PET. Therefore, the preferred alcohol solvent is 1.4-butanediol.

[0059] Preferably, in step S3, the polycondensation catalyst includes at least one of butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds, titanium-magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide.

[0060] Preferably, in step S3, the amount of the polycondensation catalyst added is 0.03-0.1 wt.% of the waste polyester.

[0061] Preferably, in step S3, the temperature of the polycondensation reaction is 240-250° C., the time is 2-5 hours, and the pressure is 20-100 Pa.

[0062] Preferably, in step S3, the stabilizer is one or more of organic phosphites, trimethyl phosphates, and hindered phenols.

[0063] Optionally, the organic phosphite stabilizer may be one or more of trimethyl phosphite, triethyl phosphite or triphenyl phosphite.

[0064] Optionally, the phosphate stabilizer may be one or more of triphenyl phosphate, trimethyl phosphate or triethyl phosphate.

[0065] Optionally, the hindered phenol stabilizer may be 3,5-di-tert-butyl-4-hydroxybenzyl diethylphosphonate (antioxidant 1222) and / or antioxidant 1010.

[0066] Preferably, in step S1, the microwave reaction conditions are as follows: frequency 2450 Hz, temperature 180-230° C., and time 20-120 min.

[0067] Preferably, in step S2, the microwave reaction conditions are as follows: frequency of 2450 Hz, temperature of 160-190° C., and time of 10-20 min.

[0068] In addition, the present invention also provides an application of the PBET copolyester in toys and precision instruments.

[0069] Compared with the prior art, the present invention has the following beneficial effects:

[0070] The present invention develops a PBET copolyester and a preparation method thereof. The PBET copolyester of the present invention uses waste polyester as a raw material, and is prepared through the steps of primary depolymerization, re-depolymerization and polycondensation to obtain a PBET copolyester with low heavy metal content and suitable crystallinity.

[0071] The initial depolymerization and the re-depolymerization are carried out under microwave conditions, wherein the re-depolymerization includes the addition of a chelating agent, and the addition of the chelating agent and the re-depolymerization reaction synergistically remove most of the metal ion residues in the waste polyester, and the obtained PBET copolyester has an extremely low heavy metal content, wherein the zinc content is ≤100ppm, and the titanium content is ≤120ppm.

[0072] The PBET copolyester of the present invention utilizes waste polyester, including electronic pallet materials, bottle materials and textiles, effectively reduces the use of petroleum resources and reduces waste generation; improves the utilization rate of waste polyester; the produced product PBET copolyester has the advantages of PBT and PET, has the characteristics of nylon and spandex fibers when used as fibers, and is closer to the excellent performance of natural fibers such as cotton, linen, wool, silk, etc.; has excellent physical and mechanical properties when used as engineering plastics, has high impact resistance, and has low mold shrinkage and good dimensional stability, and can be widely used in industrial and civil fields such as electronics and electrical, machinery manufacturing, automobiles, instruments, aviation, household appliances, sporting goods, children, toys, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0073] Figure 1 is the infrared spectrum of the PBET copolyester of Example 1;

[0074] Figure 2 is the H NMR spectrum of the PBET copolyester of Example 1;

[0075] Figure 3 This is the XRD pattern of the PBET copolyester of Example 1. DETAILED DESCRIPTION

[0076] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form.

[0077] The raw materials in the embodiments and comparative examples of the present invention can be obtained from commercial sources;

[0078] in:

[0079] Waste polyester-1, PET, recycled from electronic pallet materials;

[0080] Waste polyester-2, PBT, recycled from Changchun, Taiwan, single glass fiber reinforced PBT product waste;

[0081] Waste polyester-3, OBP-PET, YH002, recycled from Yonghong Recycling Resources Co., Ltd.;

[0082] Depolymerization catalyst and polycondensation catalyst: butyl titanate, purchased from Aladdin;

[0083] Depolymerization catalyst: zinc acetate, purchased from Aladdin;

[0084] Chelating agents: chitosan, activated carbon, lignin, and phytic acid were purchased from Maclean;

[0085] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.

[0086] Examples 1 to 3

[0087] Examples 1 to 3 respectively provide a method for preparing a PBET copolyester, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 1:

[0088] S1. Initial depolymerization:

[0089] The waste polyester with an average particle size of ≤2 mm was dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction in a nitrogen atmosphere and microwave conditions (microwave frequency 2450 Hz) to obtain a primary depolymerization product;

[0090] S2. Re-depolymerization:

[0091] Extracting part of the diol from the primary depolymerization product obtained in step S1 by vacuum distillation, adding a chelating agent, placing the product in a microwave reactor, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions (microwave frequency 2450 Hz), and filtering the reactant to obtain a filtrate as the re-depolymerization product;

[0092] S3. Polycondensation:

[0093] After removing excess alcohol from the re-depolymerization product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, triphenyl phosphate, and subjected to a polycondensation reaction under vacuum conditions to obtain the PBET copolyester.

[0094] Table 1 Raw materials and reaction conditions of Examples 1 to 3

[0095]

[0096] Embodiments 4 to 10

[0097] Examples 4 to 10 provide a method for preparing PBET copolyester. Except for step S2, the other steps are the same as those of Example 1. Specifically, the preparation methods of Examples 4 to 10 differ from those of Example 1 in that:

[0098] In Example 4, the chelating agent is activated carbon, and the alcoholysis agent is 1,3-butanediol;

[0099] In Example 5, the type of chelating agent is lignin;

[0100] In Example 6, the type of chelating agent is phytic acid;

[0101] In Example 7, the proportion of the chelating agent to the waste polyester is 0.01 wt.%;

[0102] In Example 8, the proportion of the chelating agent to the waste polyester is 0.1 wt.%;

[0103] The conditions for the re-depolymerization reaction in Example 9 were 190° C., 10 min;

[0104] The conditions for the re-depolymerization reaction in Example 10 are 160° C., 20 min.

[0105] The monomer contents prepared in Examples 4-10 are shown in Table 2

[0106] Table 2 Monomer content of PBET copolyesters prepared in Examples 4-10

[0107]

[0108] Comparative Examples 1 to 5

[0109] Comparative Examples 1 to 5 provide a method for preparing a PBET copolyester, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 3:

[0110] S1. Initial depolymerization:

[0111] The waste polyester with an average particle size of ≤2 mm was dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction in a nitrogen atmosphere and microwave conditions (microwave frequency 2450 Hz) to obtain a primary depolymerization product;

[0112] S2. Re-depolymerization:

[0113] Extracting part of the diol from the primary depolymerization product obtained in step S1 by vacuum distillation, adding a chelating agent (or not adding a chelating agent), placing the product in a microwave reactor, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions (microwave frequency 2450 Hz), and filtering the reactants to obtain a filtrate as the re-depolymerization product;

[0114] S3. Polycondensation:

[0115] After removing excess alcohol from the re-depolymerization product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, triphenyl phosphate, and subjected to a polycondensation reaction under vacuum conditions to obtain the PBET copolyester.

[0116] Table 3 Raw materials and reaction conditions of Comparative Examples 1 to 5

[0117]

[0118]

[0119] Performance Testing

[0120] The performance test of the PBET copolyesters prepared in the above examples and comparative examples is carried out as follows:

[0121] Melting point: ISO 11357-3:2018;

[0122] Relative viscosity: According to the GB / T 17931-1999 standard method, it is measured in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05℃, and the sample concentration is 5mg / ml;

[0123] Terminal carboxyl content: FZ / T 50012-2006;

[0124] Metal ion residue: US EPA 6010C:2014;

[0125] Crystallinity: JY / T 0587-2020;

[0126] Izod beam notched impact strength: GB / T1843-2008, impact energy 2.75kJ.

[0127] Mould shrinkage: Tested in accordance with GB / T 17037.4-2003.

[0128] The PBET copolyester prepared in Example 1 was subjected to infrared spectroscopy, nuclear magnetic hydrogen spectrum, and XRD detection, and the specific method was as follows:

[0129] Infrared spectrum: The sample preparation method adopts hot pressing film, and the wave number range is 4000~400cm -1 , Scan times: 16, resolution: 4, sampling method: transmission;

[0130] H-NMR spectrum: Deuterated trifluoroacetic acid was used as solvent and tetramethylsilane (TMS) was used as internal standard to test H-NMR spectrum;

[0131] XRD: X-ray diffractometer (XRD) was used according to standard JY / T 0587-2020.

[0132] Using XRD testing, the crystallization peak (sharp peak) and non-crystallization peak area (diffuse peak) are obtained, and the crystallinity is calculated according to the following formula:

[0133]

[0134] Where:

[0135] Wc-crystallinity

[0136] I C -Integrated area of ​​diffraction peak in crystalline state

[0137] I a -Integrated area of ​​diffraction peak of amorphous state

[0138] The infrared spectrum of the PBET copolyester of Example 1 is shown in Figure 1 , NMR hydrogen spectrum see Figure 2 , XRD pattern see Figure 3 .

[0139] The test results of the embodiment are shown in Table 4, and the test results of the comparative example are shown in Table 5, wherein the mold shrinkage is evaluated for the ABS / PBET alloy with a PBET content of 35%. 65 parts of ABS (grade PA757) resin, 35 parts of PBET resin, 0.2 parts of antioxidant (antioxidant 1076 and antioxidant 168 are compounded in a mass ratio of 1:1) and 0.2 parts of weathering agent (UV770) are uniformly mixed, and then melt-mixed and extruded and granulated at 230-245° C. using a twin-screw extruder to obtain the ABS / PBET alloy.

[0140] Table 4

[0141]

[0142] Table 5

[0143]

[0144]

[0145] From the test results in Table 4, it can be seen that the metal ion content of the PBET copolyester prepared by each embodiment of the present invention using recycled PBT and PET as raw materials is extremely low, wherein the zinc ion content of some embodiments is ≤70ppm, the titanium ion content is ≤85ppm, and the calcium ion content is ≤35ppm. At the same time, the PBET copolyester prepared by each embodiment of the present invention also has good dimensional stability and excellent toughness, and the Izod notched impact strength is ≥4.0KJ / m 2 .

[0146] According to Examples 1, 4 to 6, it can be seen that when phytic acid is used as a chelating agent, the metal ion content of the PBET copolyester is relatively lower, the Izod notched impact strength is relatively higher, and the PBET copolyester has excellent mechanical properties. According to the test results of the comparative examples, in Comparative Examples 1 and 2, without adding a chelating agent, the metal ion content of the obtained PBET copolyester is very high, and the excessively high residual amount of metal ions also deteriorates the toughness of the PBET copolyester, and the mold shrinkage of Comparative Examples 1-2 is relatively high, that is, the dimensional stability decreases.

[0147] According to the test results of Comparative Examples 3 and 4, it can be seen that in the re-depolymerization process of step S2, when the re-depolymerization temperature is greater than 190°C and when the re-depolymerization temperature is less than 160°C, the removal effect of metal ions is poor and the residual amount of metal ions is high; and the mold shrinkage rates of the products obtained in Comparative Examples 3-4 all show an increasing trend, that is, the dimensional stability decreases, and the mold shrinkage rate of Comparative Example 5 is high because of its high crystallinity.

[0148] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A PBET copolyester, characterized in that: The PBET copolyester is derived from repeating units of the following components: Component A: aromatic dicarboxylic acid; Component B: based on the total molar amount of component B, comprising 60 to 96 mol% of 1,4-butanediol or 1,3-butanediol and 4 to 40 mol% of ethylene glycol; The crystallinity of the PBET copolyester is 5-20%, the zinc content in the PBET copolyester is ≤100ppm, and the titanium content is ≤120ppm.

2. The PBET copolyester according to claim 1, characterized in that The melting point of the PBET copolyester is 200-220°C.

3. The PBET copolyester according to claim 1, characterized in that The relative viscosity of the PBET copolyester is 1.4 to 1.

8.

4. The PBET copolyester according to claim 1, characterized in that The terminal carboxyl content of the PBET copolyester is 20 to 37 mmol / t.

5. The PBET copolyester according to claim 1, characterized in that: The zinc content in the PBET copolyester is 35-70 ppm, and the titanium content is 40-85 ppm.

6. The method for preparing the PBET copolyester according to any one of claims 1 to 5, characterized in that: The steps include: S1. Initial depolymerization: Dissolving the waste polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product; The waste polyester includes one or more of recycled polyethylene terephthalate, polybutylene terephthalate, and PET / PBT alloy; The temperature of the initial depolymerization reaction is 180-230°C and the time is 20-120 minutes; S2. Re-depolymerization: Extracting part of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions, and filtering the reactant to obtain a filtrate as the re-depolymerization product; The temperature of the re-depolymerization reaction is 160-190°C and the time is 10-20 minutes; S3. Polycondensation: After removing excess alcohol from the re-depolymerization product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, and subjected to a polycondensation reaction under vacuum conditions until the relative viscosity is 1.4 to 1.8, thereby obtaining the PBET copolyester.

7. The preparation method according to claim 6, characterized in that: In step S2, the chelating agent includes at least one of chitosan, activated carbon, lignin, and phytic acid, preferably phytic acid.

8. The preparation method according to claim 6, characterized in that: In step S2, the amount of the chelating agent added is 0.01-0.1 wt.% of the waste polyester.

9. The preparation method according to claim 6, characterized in that: Includes at least one of the following features (a) to (c): (a) The depolymerization catalyst comprises at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate; (b) When the waste polyester contains PET, the alcohol solvent contains 1,4-butanediol or 1,3-butanediol; when the waste polyester contains PBT, the alcohol solvent contains ethylene glycol; (c) The polycondensation catalyst includes at least one of butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds, titanium-magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide.

10. Use of the PBET copolyester according to any one of claims 1 to 5 in the preparation of toys and precision instruments.

Citation Information

Patent Citations

  • Preparation method of 1,3-butanediol modified PBTPET (Polybutylece Terephthalate Polyethylene Terephthalate) copolymer fiber

    CN101824140A

  • Improved process for the preparation of modified poly(alkylene terephthalate) employing an in-situ titanium-containing catalyst

    CN105452330A

  • Low-shrinkage high-strength polyester industrial yarn and preparation method thereof

    CN105646856A

  • Amorphous copolyester and preparation method thereof

    CN106866948A

  • Continuous preparation method of biodegradable block co-polyester and biodegradable block co-polyester

    CN112745489A