Titanium polyester polycondensation catalyst and preparation method thereof
By using a titanium-based polyester polycondensation catalyst composed of water-soluble organic titanium, phosphate, triethanolamine and metal organic salt, combined with sulfonic acid synergistic catalysis, the problems of low activity and poor hydrolysis stability of titanium-based catalysts are solved, and polyester is realized It has a high-efficiency and environmentally friendly catalytic effect in synthesis, suitable for industrial production.
Patent Information
- Application Number
- CN202411091108.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing titanium catalysts are relatively low in polyester synthesis, have poor hydrolysis stability and many side reactions, resulting in a wide distribution of molecular weight, poor mechanical properties and chromatics, and are complex in preparation process and high cost, making it difficult to produce on a large scale in industrial production. .
Titanium-based polyester polycondensation catalyst composed of water-soluble organic titanium, phosphate, triethanolamine, metal organic salts and organic solvents is prepared through a specific stirring and heating process, and sulfonic acid is added to synergistically catalyze to improve the activity and selectivity of the catalyst. , reduce raw material consumption, simplify the preparation process, and avoid high temperature and high vacuum conditions and the generation of waste gas and waste liquid.
The high activity and good selectivity of the catalyst are achieved, the polyester polycondensation reaction time is shortened, the molecular weight distribution and hue of the product is improved, the raw material consumption is reduced, the preparation process is simplified, and the preparation process is suitable for industrial production, and the production of waste is reduced.
Smart Images

Figure BDA0004986605170000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of chemical catalysts, in particular to a polycondensation catalyst in polyester synthesis. Technical Background
[0002] Polyester catalytic systems are divided into antimony, titanium and germanium. Antimony catalyst systems are gradually abandoned due to their eco-toxicity, and germanium catalyst systems are difficult to apply on a large scale in industry due to their high cost. Titanium catalyst systems are green, environmentally friendly and cheap, and have been widely used in the polyester synthesis industry. At present, there are still some problems with the titanium catalyst system used for industrial production of polyester, such as: the catalyst activity is low and cannot meet the needs of polyester synthesis production; the highly active titanium catalyst causes local overreaction and the molecular weight distribution of polyester products is wide; the catalyst selectivity is poor, there are many side reactions, and the mechanical properties and color of the product are poor.
[0003] Alkyl titanium oxides such as tetrabutyl titanate and tetraisopropyl titanate and other highly active titanium catalysts have been used in the industrial production of polyester. Since polyester raw materials contain a certain amount of water and a large amount of water is produced during the esterification process, the hydrolysis of alkyl titanium oxides is caused, resulting in the production of titanium dioxide or titanium polymers and precipitation and inactivation. In order to inhibit the hydrolysis of the catalyst during the polyester synthesis process, the British Imperial Chemical Company (CN1610580A) used hydroxycarboxylic acids as complexes to react with titanates, and the resulting modified titanium catalysts were stable to water. DuPont (CN1402653A) also proposed to react multifunctional organics (such as polyol amines, hydroxycarboxylic acids, polycarboxylic acids, condensed polycarboxylic acids) with titanates to improve the hydrolysis stability of titanates. Patents CN1796434A and CN102453249A disclose a method for preparing a catalyst of a rare earth compound and a titanium compound mixture. The catalytic system can significantly increase the reaction rate and product molecular weight, and improve the yellowing of the resin; however, the rare earth resources in the catalyst of the patent are expensive, and the preparation method is relatively complicated, making it difficult to prepare in large quantities industrially. Patent CN103333328A discloses a method for preparing a silicon-titanium composite catalyst, which can shorten the reaction cycle, and the prepared polyester has good hue and high molecular weight; however, the catalyst preparation process uses high temperature and high vacuum conditions, which has high requirements on equipment, and produces waste gas and waste liquid during the preparation process. Summary of the invention
[0004] The invention provides a titanium polyester polycondensation catalyst and a preparation method thereof. The catalyst has low cost, controllable activity, and a simple and environmentally friendly preparation process.
[0005] In order to achieve the above object, the present invention provides a titanium polyester polycondensation catalyst, which adopts the following technical scheme:
[0006] A titanium polyester polycondensation catalyst comprises the following components in parts by weight: 1-10 parts of water-soluble organic titanium, 0.2-5 parts of phosphate ester, 1-3 parts of triethanolamine, 1-5 parts of metal organic salt and 5-50 parts of organic solvent.
[0007] The water-soluble organic titanium is one of di(triethanolamine)titanate diisopropyl ester and ammonium lactate titanium salt or a mixture thereof.
[0008] The phosphate ester is one of triphenyl phosphate, tris(trimethylsilyl)phosphate or glycerol phosphate or a mixture thereof.
[0009] The metal organic salt is one of organic salts of potassium, zinc or zirconium or a mixture thereof.
[0010] The organic solvent is one of ethylene glycol, 1,3-propylene glycol or 1,4-butanediol or a mixture thereof.
[0011] A titanium polyester polycondensation catalyst also contains 0.1 to 3 parts by weight of sulfonic acid. Sulfonic acid is a water-soluble strong acid organic compound with certain polyester polycondensation catalytic activity. Sulfonic acid can play a synergistic catalytic role with water-soluble organic titanium to further improve the activity of the catalyst.
[0012] The sulfonic acid is p-toluenesulfonic acid or dodecylbenzenesulfonic acid or a mixture thereof.
[0013] In order to achieve the above object, the present invention provides a method for preparing a titanium-based polyester polycondensation catalyst, which adopts the following technical scheme:
[0014] 1) heating the organic solvent to 60-100° C., slowly adding triethanolamine and phosphate while stirring, and stirring at 60-100° C. for 20-60 minutes to obtain a first mixture;
[0015] 2) Adding water-soluble organic titanium and metal organic salt to the first mixture, stirring at 40-100° C. for 20-120 minutes to obtain a polyester polycondensation catalyst.
[0016] In order to achieve the above object, the present invention provides a method for preparing a titanium polyester polycondensation catalyst, and also has the following technical scheme:
[0017] 1) heating the organic solvent to 60-120° C., slowly adding sulfonic acid while stirring, and after the addition is completed, continuing to stir for 30-60 minutes to obtain a first mixture;
[0018] 2) adding triethanolamine and phosphate to the first mixture, stirring at 60-100° C. for 20-60 minutes to obtain a second mixture;
[0019] 3) adding water-soluble organic titanium and metal organic salt to the second mixture, stirring at 40-100° C. for 20-120 minutes to obtain a polyester polycondensation catalyst.
[0020] The beneficial effects brought by the present invention are as follows: First, the present invention uses water-soluble organic titanium as an active component, metal organic salt as a co-active component, phosphate ester as a stabilizer, and triethanolamine as a complexing agent, which solves the problems of poor hydrolysis stability of the catalyst and many side reactions, so that the catalyst has high activity and good selectivity, reduces the raw material consumption in the polyester production process, and improves the yellowing phenomenon of the polyester product. Secondly, if sulfonic acid is added to the titanium-based polyester polycondensation catalyst of the present invention, it can play a synergistic catalytic role with the water-soluble organic titanium to further improve the activity of the catalyst. The titanium-based polyester polycondensation catalyst of the present invention is suitable for the field of polyester synthesis.
[0021] The catalyst of the present invention does not contain expensive elements such as rare earth, and the raw materials are cheap and easily available; the catalyst preparation does not need to be carried out under high temperature and high vacuum conditions, and no waste gas or waste liquid is generated. The preparation method is simple and environmentally friendly, and is conducive to large-scale production. DETAILED DESCRIPTION
[0022] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary illustrations and explanations of the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope of protection of the present invention.
[0023] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0024] The present invention is further described in detail below with reference to specific embodiments.
[0025] Polyester polycondensation catalyst examples
[0026] Example 1
[0027] Components in parts by weight: 1 part of di(triethanolamine) diisopropyl titanate, 0.2 parts of triphenyl phosphate, 1 part of triethanolamine, 1 part of zinc acetate and 8 parts of ethylene glycol.
[0028] Example 2
[0029] Components in parts by weight: 5 parts of di(triethanolamine)diisopropyl titanate, 2 parts of triphenyl phosphate, 3 parts of triethanolamine, 1 part of zinc acetate, 1 part of potassium isooctanoate and 25 parts of ethylene glycol.
[0030] Example 3
[0031] Components in parts by weight: 5 parts of di(triethanolamine)diisopropyl titanate, 5 parts of ammonium lactate titanium salt, 1 part of triphenyl phosphate, 4 parts of tri(trimethylsilyl) phosphate, 2 parts of triethanolamine, 2 parts of potassium isooctanoate and 50 parts of ethylene glycol.
[0032] Example 4
[0033] Components in parts by weight: 2 parts of di(triethanolamine)diisopropyl titanate, 4 parts of ammonium lactate titanium salt, 5 parts of tri(trimethylsilyl)phosphate, 2 parts of triethanolamine, 3 parts of potassium isooctanoate and 28 parts of propylene glycol.
[0034] Example 5
[0035] Components in parts by weight: 4 parts of ammonium titanium lactate, 1 part of tris(trimethylsilyl)phosphate, 1 part of glycerophosphate, 1 part of triethanolamine, 1 part of zinc isooctanoate, 5 parts of ethylene glycol and 15 parts of propylene glycol.
[0036] Example 6
[0037] Components in parts by weight: 6 parts of di(triethanolamine)diisopropyl titanate, 3 parts of ammonium lactate titanium, 3 parts of tri(trimethylsilyl) phosphate, 3 parts of triethanolamine, 2 parts of zinc isooctanoate, 3 parts of zirconium isooctanoate, 30 parts of propylene glycol and 10 parts of butanediol.
[0038] Example 7
[0039] Components in parts by weight: 7 parts of ammonium titanium lactate, 1 part of glycerophosphate, 3 parts of triethanolamine, 1 part of zinc acetate, 1 part of zirconium isooctanoate, 35 parts of butanediol, 2 parts of p-toluenesulfonic acid and 1 part of dodecylbenzenesulfonic acid.
[0040] Example 8
[0041] Components in parts by weight: 1 part of di(triethanolamine)diisopropyl titanate, 9 parts of ammonium lactate titanium salt, 5 parts of glycerophosphate, 3 parts of triethanolamine, 1 part of zirconium isooctanoate, 25 parts of ethylene glycol, 25 parts of butanediol and 0.1 parts of p-toluenesulfonic acid.
[0042] Comparative Example 1
[0043] Comparative Example 1 was designed according to Example 1, and the components in parts by weight were: 1 part of tetrabutyl titanate, 0.2 parts of triphenyl phosphate, 1 part of triethanolamine, 1 part of zinc acetate and 8 parts of ethylene glycol.
[0044] Comparative Example 2
[0045] Comparative Example 2 was designed according to Example 5, and the components in parts by weight were: 9 parts of tetraisopropyl titanate, 1 part of tris(trimethylsilyl) phosphate, 1 part of glycerophosphate, 1 part of triethanolamine, 1 part of zinc isooctanoate, 5 parts of ethylene glycol and 15 parts of propylene glycol.
[0046] The following is an example of a method for preparing a catalyst:
[0047] Example 9
[0048] Taking the preparation of the catalysts of Examples 1 to 3 as an example, an organic solvent was weighed and added to a round-bottom flask, heated to 60°C, triethanolamine and phosphate were slowly added while stirring, and stirring was continued for 60 minutes after the addition was completed to obtain a first mixture; water-soluble organic titanium and metal organic salt were added to the first mixture, heated to 100°C, and stirred at 100°C for 120 minutes to obtain polyester condensation catalysts, recorded as CAT-1, CAT-2 and CAT-3.
[0049] Example 10
[0050] Taking the preparation of the catalysts of Examples 4 to 6 as an example, an organic solvent was weighed and added to a round-bottom flask, heated to 100°C, triethanolamine and phosphate were slowly added while stirring, and stirring was continued for 20 minutes after the addition was completed to obtain a first mixture; water-soluble organic titanium and metal organic salt were added to the first mixture, the temperature was reduced to 60°C, and stirred at 60°C for 60 minutes to obtain polyester condensation catalysts, recorded as CAT-4, CAT-5 and CAT-6.
[0051] Embodiment 11
[0052] Taking the preparation of the catalysts of Examples 7 to 8 as an example, an organic solvent was weighed and added to a round-bottom flask, heated to 60°C, and sulfonic acid was slowly added while stirring. After the addition was completed, stirring was continued for 30 minutes to obtain a first mixture; triethanolamine and phosphate were added to the first mixture, heated to 100°C, and stirred at 100°C for 40 minutes to obtain a second mixture; water-soluble organic titanium and metal organic salt were added to the second mixture, cooled to 70°C, and stirred at 70°C for 120 minutes to obtain polyester condensation catalysts, recorded as CAT-7 and CAT-8.
[0053] The preparation of the catalyst in Comparative Example 1 is similar to that of CAT-1, except that the organic titanium used is tetrabutyl titanate.
[0054] The preparation of the catalyst in Comparative Example 2 is similar to that of CAT-5, except that the organic titanium used is tetraisopropyl titanate.
[0055] The eight catalysts CAT-1, CAT-2, CAT-3, CAT-4, CAT-5, CAT-6, CAT-7, CAT-8 prepared by the above process and the two catalysts of the comparative example were used to synthesize PBAT (polybutylene terephthalate-adipate). The specific test steps are as follows:
[0056] Terephthalic acid (1.8kg), 1,4-butanediol (1.76kg), and titanium catalyst (80ppm in terms of titanium element) were added to a 10L reactor, and the temperature was raised for esterification. The stirring speed was 50rpm, and the reaction was 180min starting from the water outlet of the process tower, and the esterification temperature was controlled at about 230°C. Adipic acid (1.72kg), 1,4-butanediol (1.52kg), and titanium catalyst (160ppm in terms of titanium element) were added to a 5L reactor, and the temperature was raised for esterification. The stirring speed was 50rpm, and the reaction was 90min starting from the water outlet of the process tower, and the esterification temperature was controlled at about 190°C. After the esterification was completed, the esterified product in the 5L reactor was transferred to the 10L reactor, and the co-esterification reaction was carried out for 30min, and the co-esterification temperature was controlled at about 230°C. After the co-esterification reaction was completed, vacuum polycondensation was carried out, and the vacuumization was divided into two stages: low vacuum pre-polycondensation and high vacuum final polycondensation. In the low vacuum pre-condensation stage, the kettle temperature is controlled at about 230°C, the stirring speed is 50rpm, the absolute pressure in the reactor is controlled at about 2000Pa, and the duration is 60min. In the high vacuum final condensation stage, the kettle temperature is controlled at about 230°C, the stirring speed is 50rpm, and the absolute pressure in the reactor is controlled below 100Pa. When the stirring motor power rises to 230W, the stirring is stopped, and the melt is pressed out with nitrogen, pulled into strips through a hole die, cooled in a water tank, and pelletized to obtain PBAT polyester particles. The obtained particles were tested after drying, and the results are shown in the following table:
[0057]
[0058] The basic principles, main features and advantages of the present invention are shown and described above. Compared with the comparative example, the catalytic activity of the catalyst used in the embodiment for polyester synthesis is higher, the polycondensation reaction time is significantly shortened, and the hue of the obtained polyester product is significantly improved. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic characteristics of the present invention. Therefore, from any point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. The claims should not be regarded as limiting the claims involved.
[0059] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A titanium polyester polycondensation catalyst, It is characterized in that The invention comprises the following components in parts by weight: 1 to 10 parts of water-soluble organic titanium, 0.2 to 5 parts of phosphoric acid ester, 1 to 3 parts of triethanolamine, 1 to 5 parts of metal organic salt and 5 to 50 parts of organic solvent.
2. A titanium-based polyester polycondensation catalyst according to claim 1, It is characterized in that The water-soluble organic titanium is one of di(triethanolamine)titanate diisopropyl ester and ammonium lactate titanium salt or a mixture thereof.
3. A titanium polyester polycondensation catalyst according to claim 1, It is characterized in that The phosphate ester is one of triphenyl phosphate, tris(trimethylsilyl)phosphate or glycerol phosphate or a mixture thereof.
4. A titanium polyester polycondensation catalyst according to claim 1, It is characterized in that The metal organic salt is one of organic salts of potassium, zinc or zirconium or a mixture thereof.
5. A titanium-based polyester polycondensation catalyst according to claim 1, It is characterized in that The organic solvent is one of ethylene glycol, 1,3-propylene glycol or 1,4-butanediol or a mixture thereof.
6. A titanium-based polyester polycondensation catalyst according to claim 1, It is characterized in that There are also 0.1 to 3 parts by weight of sulfonic acid.
7. A titanium polyester polycondensation catalyst according to claim 6, It is characterized in that The sulfonic acid is p-toluenesulfonic acid or dodecylbenzenesulfonic acid or a mixture thereof.
8. A method for preparing a titanium polyester polycondensation catalyst according to any one of claims 1 to 5, It is characterized in that It includes the following sequence and steps: 1) heating the organic solvent to 60-100° C., slowly adding triethanolamine and phosphate while stirring, and stirring at 60-100° C. for 20-60 minutes to obtain a first mixture; 2) Adding water-soluble organic titanium and metal organic salt to the first mixture, stirring at 40-100° C. for 20-120 minutes to obtain a polyester polycondensation catalyst.
9. A method for preparing a titanium polyester polycondensation catalyst according to any one of claims 6 or 7, It is characterized in that It includes the following sequence and steps: 1) heating the organic solvent to 60-120° C., slowly adding sulfonic acid while stirring, and after the addition is completed, continuing to stir for 30-60 minutes to obtain a first mixture; 2) adding triethanolamine and phosphate to the first mixture, stirring at 60-100° C. for 20-60 minutes to obtain a second mixture; 3) adding water-soluble organic titanium and metal organic salt to the second mixture, stirring at 40-100° C. for 20-120 minutes to obtain a polyester polycondensation catalyst.