Composite ink for 3D printing and preparation method thereof

By in situ polymerizing polyaniline on the surface of Ti3C2Tx MXene nanosheets to form PANI/MXene composites, the problems of easy oxidation and self-stacking of MXene inks are solved, and capacitance performance is improved. It is suitable for the preparation of electrodes of energy storage devices.

CN118930852APending Publication Date: 2024-11-12GUANGXI UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411118288.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Pure MXene inks are prone to oxidation and self-stacking in the air, resulting in a decline in the capacitance performance of the material and its conductivity will also decrease after adding additives, making it difficult to solve these problems.

Method used

Low-temperature chemical oxidation polymerization is used to polymerize polyaniline in situ on the surface of Ti3C2Tx MXene nanosheets to form a PANI/MXene composite, form a protective layer and improve the capacitance performance of the material.

Benefits of technology

It effectively overcomes the problems of easy oxidation and self-stacking of MXene, improves the conductivity and capacitive performance of the material, and is suitable for electrode preparation of energy storage devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930852A_ABST
    Figure CN118930852A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of 3D printing, in particular to composite ink for 3D printing and a preparation method of the composite ink. According to the specific technical scheme, according to the preparation method of the composite ink for 3D printing, a single-layer Ti < 3 > C < 2 > T < x > MXene solution is used as a dispersion, and polyaniline is formed by in-situ polymerization of aniline monomers on the surface of a Ti < 3 > C < 2 > T < x > MXene nanosheet through a low-temperature chemical oxidation polymerization method. According to the prepared composite ink, the electrochemical performance such as conductivity and specific capacitance of the material is improved, the problems that single MXene is prone to oxidation and self-stacking are solved, and the composite ink can be used for electrode preparation of energy storage devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of 3D printing, and in particular to a composite ink for 3D printing and a preparation method thereof. Background Art

[0002] 3D printing, as an emerging method for preparing electrodes, has attracted widespread attention from researchers. Among them, the preparation of printable ink is the most critical step in 3D printing. MXene is widely used in the preparation of electrode inks due to its advantages such as high conductivity, large specific surface area, excellent hydrophilicity, and adjustable functional groups. However, pure MXene ink also faces challenges: it is easy to oxidize in the air, resulting in a decrease in the capacitance performance of the material, and self-stacking causes the ink to clog the needle during printing. Therefore, it is urgent to find strategies to solve these difficulties. Many researchers have added additives such as carbon nanotubes (CNTs) and ethyl cellulose to MXene inks to adjust the viscosity of MXene inks, but this will lead to problems such as decreased conductivity of the material. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a composite ink for 3D printing and a preparation method thereof, which improves the electrochemical properties of the material such as conductivity and specific capacitance, overcomes the problems of easy oxidation and self-stacking of single MXene, and can be used for the preparation of electrodes for energy storage devices.

[0004] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0005] The present invention discloses a method for preparing a composite ink for 3D printing, using a single layer of Ti3C2T x The MXene solution was used as a dispersion, and the aniline monomer was polymerized on Ti3C2T4 by low-temperature chemical oxidation polymerization. x In situ polymerization of polyaniline on the surface of MXene nanosheets.

[0006] Preferably, the single layer Ti3C2T x The mass concentration of the MXene solution is 1-5 g / L, and the molar concentration of the aniline is 0.05M.

[0007] Preferably, the single layer Ti3C2T x The preparation process of MXene is as follows: a mixture of lithium fluoride and dilute hydrochloric acid is used as an etching solution to etch Ti3AlC2 MAX at a reaction temperature of 30±10°C. After the reaction is completed, the product is washed to neutrality and ultrasonically dispersed to obtain Ti3C2T x MXene monolayer.

[0008] Preferably, the concentration of the hydrochloric acid is 8 to 11 M, and the molar mass ratio of the lithium fluoride to Ti3AlC2 MAX is 7.5 to 12:1.

[0009] Preferably, in a single layer Ti3C2T x Perchloric acid solution is added to the MXene solution, and the solution is stirred at a temperature of -10 to 0°C. Aniline is then added and stirred, and then ammonium persulfate solution is quickly added as an oxidant. The reaction is carried out for 20 to 30 hours. After the reaction is completed, the product is washed and freeze-dried to obtain a PANI / MXene composite.

[0010] Preferably, the PANI / MXene composite is dissolved in deionized water and ground to obtain a PANI / MXene-based composite ink.

[0011] Preferably, the molar concentration of aniline is 0.05 M, the molar concentration ratio of ammonium persulfate to aniline is 1:1.5, and the solvent of the ammonium persulfate solution is 1 M perchloric acid.

[0012] Preferably, the concentration of the PANI / MXene-based composite ink is 150 to 300 mg / mL.

[0013] Correspondingly, a PANI / MXene-based composite ink prepared by the above preparation method.

[0014] The present invention has the following beneficial effects:

[0015] 1. The present invention converts Ti3C2T x MXene is composited with conductive polymer PANI. PANI in Ti3C2T x The composite on the surface of MXene nanosheets forms a protective layer, which effectively alleviates the x Oxidation phenomenon of MXene. At the same time, PANI and Ti3C2T x MXene also produces a synergistic effect to increase the capacitance of the composite material. Therefore, the composite ink preparation method disclosed in the present invention not only effectively overcomes the limitations of a single material, but also improves the capacitance and other properties of the material, and can be widely used in the preparation of electrodes for energy storage devices.

[0016] 2. The PANI / MXene-based composite ink prepared by the present invention overcomes the defects of PANI and MXene when used alone (PANI is prone to collapse when used alone as an electrode, and MXene is prone to oxidation and self-stacking when used alone). xThe polymerization on the surface of the MXene sheet forms an antioxidant film, which plays a protective role. The three-dimensional structure formed by the two reduces the ion diffusion path and produces a synergistic effect to increase the specific capacitance of the material. Therefore, PANI / MXene-based composite ink can be used in the preparation of electrodes for energy storage devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The flowchart of the preparation of PANI / MXene-based composite ink;

[0018] Figure 2 For single-layer Ti3C2T x SEM image of MXene nanosheets;

[0019] Figure 3 The SEM image of PANI / Mxene composite (the masses of MXene in a, b, and c are 9 mg, 18 mg, and 27 mg, respectively; from top to bottom are low-magnification and high-magnification electron microscopy images, respectively);

[0020] Figure 4 The viscosity and shear rate relationship curves of four concentrations of PANI / MXene-based composite inks;

[0021] Figure 5 The modulus and shear force relationship curves of four concentrations of PANI / MXene-based composite inks; (a) 150 mg / mL, (b) 200 mg / mL, (c) 250 mg / mL, and (d) 300 mg / mL. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0024] The present invention discloses a method for preparing a composite ink for 3D printing, using a single layer of Ti3C2T x The MXene solution was used as a dispersion, and the aniline monomer was polymerized on Ti3C2T4 by low-temperature chemical oxidation polymerization. x In situ polymerization of polyaniline on the surface of MXene nanosheets.

[0025] The specific preparation process is:

[0026] (1) A mixture of lithium fluoride and dilute hydrochloric acid is used as an etching solution to etch Ti3AlC2 MAX at a reaction temperature of 30±10°C. After the reaction is completed, the product is washed to neutrality and ultrasonically dispersed to obtain Ti3C2T x MXene monolayer flakes, freeze-dried to obtain a single layer of Ti3C2T x MXene aerosol. The concentration of the hydrochloric acid is 8 to 11 M, and the molar mass ratio of the lithium fluoride to the Ti3AlC2MAX is 7.5 to 12:1.

[0027] (2) In a single layer Ti3C2T x Perchloric acid solution is added to the MXene solution, and the solution is stirred at a temperature of -10 to 0°C. Aniline is then added and stirred, and then ammonium persulfate solution is quickly added as an oxidant. The reaction is carried out for 20 to 30 hours. After the reaction is completed, the product is washed and freeze-dried to obtain a PANI / MXene composite.

[0028] Wherein, the single layer Ti3C2T x The mass concentration of the MXene solution is 1-5 g / L, and the molar concentration of the aniline is 0.05 M. The molar concentration ratio of the ammonium persulfate to the aniline is 1:1.5, and the solvent of the ammonium persulfate solution is 1 M perchloric acid.

[0029] (3) The PANI / MXene composite is dissolved in deionized water and ground to obtain a PANI / MXene-based composite ink having a concentration of 150 to 300 mg / mL.

[0030] The present invention will be further described below in conjunction with specific embodiments.

[0031] Example 1

[0032] refer to Figure 1 , a method for preparing a conductive polymer PANI / MXene-based composite ink, comprising the following steps:

[0033] (1) Ti3C2T x Preparation of MXene: LiF and dilute hydrochloric acid were used as the etching solution to etch Ti3AlC2MAX. The reaction temperature was 30°C. After the reaction was completed, the product was centrifuged and washed with deionized water until the pH was neutral. Then, Ti3C2T x MXene multilayers dispersed as Ti3C2T x MXene monolayer flakes were freeze-dried at -65 to -50 °C and a vacuum degree below 40 Pa to obtain a monolayer Ti3C2T x MXene aerosol, as attached Figure 2SEM can observe Ti3C2T x MXene presents a single-layer nanosheet morphology. Specifically: 1g lithium fluoride was dissolved in 20mL 9M hydrochloric acid and stirred for 5min, then 1g Ti3AlC2MAX was added and stirred at 30℃ for 24h, and post-processing was performed after the reaction was completed.

[0034] (2) Preparation of PANI / MXene composites: Monolayer Ti3C2T x The MXene solution was added to the perchloric acid solution and stirred at a temperature of -10°C to 0°C, and then aniline was added and stirred, and then ammonium persulfate (APS) solution pre-cooled at -10°C for 20 minutes was quickly added as an oxidant and reacted for 24 hours. After the reaction, the solution was washed with deionized water by centrifugation and freeze-dried to obtain the PANI / MXene composite. Figure 3 The composite morphology is shown, Ti3C2T x Many PANI nanowires similar to small protrusions grow on the surface of MXene nanosheets. x The solute masses in the MXene solution were 9 mg, 18 mg, and 27 mg, respectively, and deionized water was 7.96 mL. Ti3C2T x The solution in the entire reaction system after the MXene solution is 1M perchloric acid. The molar concentration of aniline is 0.05M, and the molar concentration ratio of ammonium persulfate to aniline is 1:1.5. The ammonium persulfate solution is prepared by dissolving ammonium persulfate in 5mL 1M perchloric acid.

[0035] (3) Preparation of PANI / MXene-based composite ink: The prepared PANI / MXene complex was dissolved in deionized water and ground to obtain a PANI / MXene-based composite ink. Specifically: The PANI / MXene complex was dissolved in deionized water and ground for 1 to 3 hours to obtain a PANI / MXene-based composite ink, and the ink concentrations were 150 mg / mL, 200 mg / mL, 250 mg / mL, and 300 mg / mL, respectively; the viscosity and modulus parameters of the four inks were compared and applied to 3D printing, and it was found that the ink with a concentration of 300 mg / mL had the best viscosity, the best printability, and the best self-supporting property, as shown in the attached figure. Figure 4 , Figure 5 shown.

[0036] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a composite ink for 3D printing, Features: With single layer Ti 3 C 2 T x The MXene solution was dispersed and the aniline monomer was polymerized on Ti by low-temperature chemical oxidation polymerization. 3 C 2 T x In situ polymerization of polyaniline on the surface of MXene nanosheets.

2. The preparation method according to claim 1, Features: The single layer Ti 3 C 2 T x The mass concentration of the MXene solution is 1-5 g / L, and the molar concentration of the aniline is 0.05M.

3. The preparation method according to claim 1, Features: The single layer Ti 3 C 2 T x The preparation process of MXene is as follows: lithium fluoride and dilute hydrochloric acid are used as an etching solution to etch Ti 3 AlC 2 MAX is used for etching reaction at a temperature of 30±10°C. After the reaction is completed, the product is washed to neutrality and ultrasonically dispersed to obtain Ti 3 C 2 T x MXene monolayer.

4. The preparation method according to claim 3, Features: The concentration of the hydrochloric acid is 8-11M, the lithium fluoride and Ti 3 AlC 2 The molar mass ratio of MAX is 7.5 to 12:

1.

5. The preparation method according to any one of claims 1 to 4, Features: In single-layer Ti 3 C 2 T x Perchloric acid solution is added to the MXene solution, and the solution is stirred at a temperature of -10 to 0°C. Aniline is then added and stirred, and then ammonium persulfate solution is quickly added as an oxidant. The reaction is carried out for 20 to 30 hours. After the reaction is completed, the product is washed and freeze-dried to obtain a PANI / MXene composite.

6. The preparation method according to claim 5, Features: The PANI / MXene composite was dissolved in deionized water and ground to obtain the PANI / MXene-based composite ink.

7. The preparation method according to claim 5, Features: The molar concentration of the aniline is 0.05 M, the molar concentration ratio of the ammonium persulfate to the aniline is 1:1.5, and the solvent of the ammonium persulfate solution is 1 M perchloric acid.

8. The preparation method according to claim 6, Features: The concentration of the PANI / MXene-based composite ink is 150 to 300 mg / mL.

9. A PANI / MXene-based composite ink prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Polyaniline nano particle / two-dimensional layered titanium carbide composite material and low-temperature preparation method of polyaniline nano particle / two-dimensional layered titanium carbide composite material

    CN106589362A

  • Titanium carbide / polyaniline composite material and preparation method thereof

    CN106633051A

  • Polyaniline surface modified titanium carbide composite material and low-temperature preparation method thereof

    CN106674517A

  • MXene-polyaniline composite material and preparation method thereof

    CN106750277A

  • Preparation and application of composite material PANI / Ti3C2Tx

    CN107346711A