Preparation method of modified polyetherimide-based composite dielectric film

By introducing core-shell structure filler TA-ZnII@SiO2 in polyetherimide, the problem of dielectric loss and interface mismatch of polymer film capacitors at high temperatures is solved, and its energy storage performance and breakdown strength are significantly improved. Achieve stable operation at high temperatures.

CN118930857AActive Publication Date: 2024-11-12DATONG CO POLYMER (XIAN) TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411248591.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

The dielectric loss of existing polymer film capacitors increases sharply under high temperature environments, resulting in a decrease in charge and discharge efficiency. The mismatch between the nanofiller and the polymer matrix interface leads to carrier accumulation, reducing the breakdown field strength and reliability of the composite material.

Method used

The tannin metal organic frame is used as the buffer shell layer to coat hydroxyl-modified silica nanoparticles to form the core-shell structure filler TA-ZnII@SiO2, and introduce it into the polyetherimide matrix to solve the problem of interface failure. Matching problems to improve the energy storage performance of composite media.

Benefits of technology

The breakdown strength and energy storage performance of the composite medium were significantly improved. The discharge energy density of 0.3% TA-ZnII@SiO2/PEI composite film at 25℃ and 150℃ was 5.9J/cm³ and 4.6J/cm³, respectively, and the energy storage was The efficiency remained at 85.6% and 83.4%, an increase of 75.1% and 154% compared with pure PEI.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930857A_ABST
    Figure CN118930857A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a modified polyetherimide-based composite dielectric film. The preparation method comprises the following steps: step 1, preparing a tannic acid solution, preparing a zinc sulfate heptahydrate solution and preparing a silicon dioxide dispersion liquid; step 2, preparing a zinc sulfate and silicon dioxide mixed solution, and preparing a core-shell structure filler TA-ZnII coated SiO2; step 3, preparing a diamine dispersion liquid; the preparation method comprises the following steps: adding a core-shell structure filler TA-ZnII coated SiO2 filler into a diamine dispersion liquid; 4, bisphenol A type diether dianhydride is added into the diamine dispersion liquid, and polyamide acid colloid is obtained; 5, vacuumizing the polyamide acid colloid, uniformly coating the polyamide acid colloid on a glass plate, removing the solvent in the film in a high-temperature oven, preserving heat, and cooling to obtain a modified polyetherimide-based composite dielectric film; the problem of interface mismatching between the SiO2 filler and the polyetherimide matrix is solved, and the aggregation phenomenon of carriers at the interface is remarkably reduced; the breakdown strength of the composite dielectric is improved, and the energy storage performance of the polyetherimide-based dielectric is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dielectric energy storage, and in particular relates to a method for preparing a modified polyetherimide-based composite dielectric film. Background Art

[0002] Dielectric capacitors have the characteristics of high power density, low-cost manufacturing, fast charging and discharging, and safety and environmental protection. They are in huge demand in industries such as high-voltage flexible direct current transmission and new energy vehicles. The polymer film capacitors widely used in the current market use biaxially oriented polypropylene (BOPP). However, the operating temperature of BOPP film is relatively low. When the temperature exceeds 105°C, its dielectric loss will rise sharply, resulting in a rapid decrease in charging and discharging efficiency, which cannot meet the performance requirements of electronic equipment in high temperature environments. In order to ensure its stable operation at high temperatures, an additional cooling system is usually required to maintain the operating temperature of BOPP, which not only increases production costs, but also leads to an increase in the size of the equipment. Therefore, it is necessary to develop high-temperature dielectric materials with good thermal stability and excellent energy storage performance at high temperatures.

[0003] Polyetherimide (PEI) is considered to be a highly promising high-temperature dielectric material due to its high breakdown strength, excellent heat resistance, simple synthesis process and easily controllable molecular structure. Through structural design from microscopic to mesoscopic levels, the introduction of hydroxyl surface-modified SiO2 nanoparticles improves the dielectric properties and energy storage performance of the PEI matrix. However, there is an interface mismatch problem between the nanofiller and the polymer matrix, which causes the accumulation of carriers at the interface between the filler and the matrix, reducing the breakdown field strength and reliability of the composite material. Summary of the invention

[0004] In order to overcome the above-mentioned deficiencies of the prior art, the object of the present invention is to provide a method for preparing a modified polyetherimide-based composite dielectric film having higher energy storage performance.

[0005] To achieve the above object, the present invention will adopt the following scheme: A method for preparing a modified polyetherimide-based composite dielectric film comprises the following steps: Step 1, dissolving 0.02-0.06 g of tannic acid in 25-75 mL of deionized water to prepare a tannic acid solution, dissolving 0.005-0.015 g of zinc sulfate heptahydrate in 25-75 mL of deionized water to prepare a zinc sulfate heptahydrate solution, and dissolving 0.05-0.15 g of hydroxyl-modified silica nanoparticles in 50-150 mL of deionized water to prepare a silica dispersion; Step 2: Pour the zinc sulfate heptahydrate solution into the silica dispersion in step 1 and mix evenly to obtain a zinc sulfate silica mixed solution; then add the tannic acid solution into the zinc sulfate silica mixed solution and mix evenly; centrifuge and wash the mixture at 12000 rpm for multiple times; and freeze-dry to prepare a core-shell structure filler TA-Zn II @SiO2; Step 3: Dissolve 1.5-4.5 g of 4,4'-diaminodiphenyl ether required for polyetherimide in 18.3-54.9 mL of N-methyl-2-pyrrolidone solvent to obtain a diamine dispersion; then II @Add SiO2 filler into diamine dispersion and stir evenly; Step 4, weighing 4.019-12.057 g of bisphenol A diether dianhydride, and adding it to the diamine dispersion in 6 portions to obtain a polyamic acid colloid; Step 5, vacuum bubble the polyamic acid colloid, then use a scraper to evenly coat the polyamic acid colloid on a glass plate, and then place it in a high-temperature oven to remove the solvent in the film, keep it warm at 150°C for 1 hour, keep it warm at 200°C for 1 hour, keep it warm at 250°C for 1 hour, and keep it warm at 300°C for 1 hour, and after natural cooling, obtain a modified polyetherimide-based composite dielectric film.

[0006] In the step 1, the concentration of the tannic acid solution is 0.0004-0.0012 mol / L, and the concentration of the zinc sulfate heptahydrate solution is 0.0012-0.0036 mol / L.

[0007] In the step 2, when the tannic acid solution is mixed with the zinc sulfate-silicon dioxide mixed solution, it is necessary to carry out the process under ultrasonic conditions, and the ultrasonic time is 8-10s.

[0008] In the step 3, 4,4'-diaminodiphenyl ether is dispersed in N-methyl-2-pyrrolidone solvent by ultrasonication for 5-15 minutes.

[0009] In step 3, the core-shell structure filler TA-Zn is added II @The mass of SiO2 filler is 0.1%-0.5% of the total mass of 4,4'-diaminodiphenyl ether and bisphenol A diether dianhydride.

[0010] In the step 4, the amounts of bisphenol A diether dianhydride added to the diamine dispersion are 2-6 g, 1-3 g, 0.5-1.5 g, 0.3-0.9 g, 0.1-0.3 g, and 0.119-0.357 g for 6 times, and the stirring time after each addition is 10-20 min, 10-20 min, 10-20 min, 10-20 min, 20-40 min, and 60-120 min, respectively.

[0011] In the step 4, during the addition of bisphenol A diether dianhydride, mechanical stirring is maintained at a low temperature of 0-10° C. and a speed of 3000 rpm.

[0012] In the step 5, the temperature and time for removing the solvent in the film are 80-90° C. and 12-18 h respectively.

[0013] Compared with the prior art, the beneficial effects of the present invention are: The present invention aims to improve the energy storage performance of PEI-based composite dielectric films, and solve the problems of low dielectric constant and high dielectric loss in high temperature environments in current polymer matrices. In order to alleviate the problem of interface mismatch between nanofillers and polymer matrices, the present invention innovatively uses tannic acid metal organic framework as a buffer shell to reduce the interface incompatibility between the matrix and the filler, and improve the energy storage performance of the composite material.

[0014] The present invention applies core-shell structure fillers to polyetherimide to obtain a modified polyetherimide-based composite dielectric film with excellent energy storage performance; in view of the problem of insufficient dielectric constant of the polymer matrix and insulation failure caused by charge accumulation, the polyetherimide-based dielectric is carefully designed from microscopic to mesoscopic, and its dielectric properties and high-temperature energy storage capacity are deeply studied; the core of the present invention is to prepare a special core-shell structure filler, that is, on the surface of hydroxyl-modified silica (SiO2) nanoparticles, tannic acid organic metal framework (TA-Zn II ); This TA-Zn II @The introduction of SiO2 core-shell structure filler not only solves the interface mismatch problem between SiO2 filler and polyetherimide matrix, but also significantly reduces the aggregation of carriers at the interface; this series of improvements significantly improves the breakdown strength of the composite medium, thereby effectively improving the energy storage performance of polyetherimide-based dielectrics.

[0015] Preparation of core-shell TA-Zn nanoparticles by coating tannic acid metal organic frameworks on the surface of hydroxyl-modified silica nanoparticles II @SiO2 filler, followed by TA-Zn II The introduction of @SiO2 filler into the polyetherimide matrix and the introduction of tannic acid metal organic framework alleviated the interface mismatch problem between SiO2 filler and matrix, reduced the aggregation of carriers at the interface, improved the breakdown performance of the composite medium, and finally effectively improved the energy storage performance of polyetherimide-based dielectrics. The results show that 0.3% TA-Zn II@The discharge energy density of SiO2 / PEI composite film at 25℃ and 150℃ was 5.9J / cm³ and 4.6J / cm³ respectively, and the energy storage efficiency remained at 85.6% and 83.4%. Compared with pure PEI, the energy storage efficiency increased by 75.1% and 154% respectively, proving that the energy storage performance of polymer dielectrics can be improved through interface structure design strategies, providing a new reference direction for the research of energy storage dielectrics. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 TA-Zn II @SiO2 filler preparation flow chart.

[0017] Figure 2 TA-Zn II @SiO2 / PEI composite film preparation flow chart.

[0018] Figure 3 TA-Zn prepared in Example 1, Example 2, Example 3 and Comparative Example 1 II @Weibull distribution diagram of breakdown field strength of SiO2 / PEI composite film and PEI film at 25℃ and 150℃.

[0019] Figure 4 TA-Zn prepared in Example 1, Example 2, Example 3 and Comparative Example 1 II @Energy storage density and energy storage efficiency diagram of SiO2 / PEI composite film and PEI film at 25℃ and 150℃. DETAILED DESCRIPTION

[0020] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. Example

[0021] A method for preparing a modified polyetherimide-based composite dielectric film comprises the following steps: Step 1, dissolving 0.02 g of tannic acid in 25 mL of deionized water to prepare a tannic acid solution, dissolving 0.005 g of zinc sulfate heptahydrate in 25 mL of deionized water to prepare a zinc sulfate solution, and dissolving 0.05 g of hydroxyl-modified silica nanoparticles in 50 mL of deionized water to prepare a silica dispersion; The concentration of the tannic acid solution is 0.0004 mol / L, and the concentration of the zinc sulfate heptahydrate solution is 0.0012 mol / L; Step 2: Pour the zinc sulfate solution into the silica dispersion and mix evenly to obtain a zinc sulfate silica mixture, then add the tannic acid solution into the mixture and mix evenly, the mixing needs to be carried out under ultrasonic conditions, and the ultrasonic time is 8s, and the mixture is centrifuged and washed multiple times at a speed of 12000rpm, and freeze-dried to prepare a core-shell structure filler TA-ZnII @SiO2; Step 3: Dissolve 1.5 g of 4,4'-diaminodiphenyl ether required for polyetherimide in 18.3 mL of N-methyl-2-pyrrolidone solvent and ultrasonicate for 5 min to obtain a diamine dispersion; then II @SiO2 filler is added to the diamine dispersion and stirred evenly. TA-Zn II @The mass of SiO2 filler is 0.1% of the total mass of 4,4'-diaminodiphenyl ether and bisphenol A diether dianhydride; Step 4, weighing 4.019 g of bisphenol A diether dianhydride, adding it to the diamine dispersion in 6 times, maintaining a low temperature of 0° C., and mechanically stirring at a speed of 3000 rpm; the added amounts were 2 g, 1 g, 0.5 g, 0.3 g, 0.1 g, and 0.119 g, respectively, and the stirring time after each addition was 10 min, 10 min, 10 min, 10 min, 20 min, and 60 min, respectively, to obtain a polyamic acid colloid; Step 5, vacuum bubble the polyamic acid colloid, then use a scraper to evenly coat the polyamic acid colloid on a glass plate, and then place it in a high-temperature oven at 80°C to remove the solvent in the film for 12 hours, keep it warm at 150°C for 1 hour, keep it warm at 200°C for 1 hour, keep it warm at 250°C for 1 hour, and keep it warm at 300°C for 1 hour, and then cool it naturally to obtain a modified polyetherimide-based composite dielectric film.

[0022] Figure 1 Example 1TA-Zn II @SiO2 filler preparation flow chart.

[0023] Figure 2 Example 1TA-Zn II @SiO2 / PEI composite film preparation flow chart. Example

[0024] A method for preparing a modified polyetherimide-based composite dielectric film comprises the following steps: Step 1, taking 0.04 g of tannic acid and dissolving it in 50 mL of deionized water to prepare a tannic acid solution, taking 0.01 g of zinc sulfate heptahydrate and dissolving it in 50 mL of deionized water to prepare a zinc sulfate solution, and dissolving 0.1 g of hydroxyl-modified silica nanoparticles in 100 mL of deionized water to prepare a silica dispersion; The concentration of the tannic acid solution is 0.0008 mol / L, and the concentration of the zinc sulfate heptahydrate solution is 0.0024 mol / L; Step 2: Pour the zinc sulfate solution into the silica dispersion and mix evenly to obtain a zinc sulfate silica mixture, then add the tannic acid solution into the mixture and mix evenly, the mixing needs to be carried out under ultrasonic conditions, and the ultrasonic time is 9s, centrifuge and wash multiple times at a speed of 12000rpm, and freeze-dry to prepare a core-shell structure filler TA-Zn II @SiO2; Step 3: Dissolve 3 g of 4,4'-diaminodiphenyl ether required for polyetherimide in 36.6 mL of N-methyl-2-pyrrolidone solvent and perform ultrasonication for 10 min to obtain a diamine dispersion; then II @SiO2 filler is added to the diamine dispersion and stirred evenly. TA-Zn II @The mass of SiO2 filler is 0.3% of the total mass of 4,4'-diaminodiphenyl ether and bisphenol A diether dianhydride.

[0025] Step 4, weighing 8.038 g of bisphenol A diether dianhydride, adding it to the diamine dispersion in 6 times, maintaining a low temperature of 5° C., and mechanically stirring at a speed of 3000 rpm; the added amounts were 4 g, 2 g, 1 g, 0.6 g, 0.2 g, and 0.238 g, respectively, and the stirring time after each addition was 15 min, 15 min, 15 min, 15 min, 30 min, and 90 min, respectively, to obtain a polyamic acid colloid; Step 5, vacuum bubble the polyamic acid colloid, then use a scraper to evenly coat the polyamic acid colloid on a glass plate, and then place it in a high-temperature oven at 85°C to remove the solvent in the film for 16 hours, keep it warm at 150°C for 1 hour, keep it warm at 200°C for 1 hour, keep it warm at 250°C for 1 hour, and keep it warm at 300°C for 1 hour, and then cool it naturally to obtain a modified polyetherimide-based composite dielectric film. Example

[0026] A method for preparing a modified polyetherimide-based composite dielectric film comprises the following steps: Step 1, taking 0.06 g of tannic acid and dissolving it in 75 mL of deionized water to prepare a tannic acid solution, taking 0.015 g of zinc sulfate heptahydrate and dissolving it in 75 mL of deionized water to prepare a zinc sulfate solution, and dissolving 0.15 g of hydroxyl-modified silica nanoparticles in 150 mL of deionized water to prepare a silica dispersion; The concentration of the tannic acid solution is 0.0012 mol / L, and the concentration of the zinc sulfate heptahydrate solution is 0.0036 mol / L; Step 2: Pour the zinc sulfate solution into the silica dispersion and mix evenly to obtain a zinc sulfate silica mixture, then add the tannic acid solution into the mixture and mix evenly, the mixing needs to be carried out under ultrasonic conditions, and the ultrasonic time is 10s, and the mixture is centrifuged and washed multiple times at a speed of 12000rpm, and freeze-dried to prepare a core-shell structure filler TA-Zn II @SiO2; Step 3: 4.5 g of 4,4'-diaminodiphenyl ether required for polyetherimide was dissolved in 54.9 mL of N-methyl-2-pyrrolidone solvent and ultrasonicated for 15 min to obtain a diamine dispersion; then TA-Zn II @SiO2 filler is added to the diamine dispersion and stirred evenly. TA-Zn II @The mass of SiO2 filler is 0.5% of the total mass of 4,4'-diaminodiphenyl ether and bisphenol A diether dianhydride; Step 4, weighing 12.057 g of bisphenol A diether dianhydride, adding it to the diamine dispersion in 6 times, maintaining a low temperature of 10° C., and mechanically stirring at a speed of 3000 rpm; the added amounts were 6 g, 3 g, 1.5 g, 0.9 g, 0.3 g, and 0.357 g, respectively, and the stirring time after each addition was 20 min, 20 min, 20 min, 20 min, 40 min, and 120 min, respectively, to obtain a polyamic acid colloid; Step 5, vacuum bubble the polyamic acid colloid, then use a scraper to evenly coat the polyamic acid colloid on a glass plate, and then place it in a high-temperature oven at 90°C to remove the solvent in the film for 18 hours, keep it warm at 150°C for 1 hour, keep it warm at 200°C for 1 hour, keep it warm at 250°C for 1 hour, and keep it warm at 300°C for 1 hour, and then cool it naturally to obtain a modified polyetherimide-based composite dielectric film.

[0027] Comparative Example 1 No addition of core-shell filler TA-Zn during the synthesis of polyetherimide II @SiO 2, The preparation of pure polyetherimide comparison sample is as follows: Step 1, dissolving 1.5 g of 4,4'-diaminodiphenyl ether in 18.3 mL of N-methyl-2-pyrrolidone solvent and ultrasonicating for 5 min to obtain a diamine dispersion; Step 2, weighing 4.019 g of bisphenol A diether dianhydride, adding it to the diamine dispersion in 6 times, and maintaining mechanical stirring at a low temperature of 3000 rpm; the added amounts were 2 g, 1 g, 0.5 g, 0.3 g, 0.1 g, and 0.119 g, respectively, and the stirring time after each addition was 10 min, 10 min, 10 min, 10 min, 20 min, and 60 min, respectively, to obtain a polyamic acid colloid; Step 3, vacuum bubble the polyamic acid colloid, then use a scraper to evenly coat the polyamic acid colloid on a glass plate, and then place it in a high-temperature oven at 80°C to remove the solvent in the film for 12 hours, keep it warm at 150°C for 1 hour, keep it warm at 200°C for 1 hour, keep it warm at 250°C for 1 hour, and keep it warm at 300°C for 1 hour, and then naturally cool it to obtain a polyetherimide film.

[0028] Figure 3 TA-Zn prepared in Example 1, Example 2, Example 3 and Comparative Example 1 II @ Weibull distribution of breakdown field strength of SiO2 / PEI composite film and PEI film at 25℃ and 150℃. II @SiO2 filler, compared with pure PEI film, the breakdown field strength of the composite film has been significantly improved at both room temperature and high temperature. Since the SiO2 core layer has high insulation performance and wide bandgap, and the buffering method of the dielectric constant of the core-shell structure decreasing layer by layer avoids stress concentration in the material, the design of the SiO2 core layer can effectively improve the breakdown field strength of the composite material. Among them, at 25℃ and 150℃, the component with the highest breakdown field strength is the 0.3% composite film, and its breakdown field strength is 619kV / mm and 599kV / mm at room temperature and high temperature, respectively. Compared with the pure PEI film at room temperature of 507kV / mm and high temperature of 505kV / mm, its breakdown field strength is increased by 22.1% and 18.6%, respectively.

[0029] Figure 4 TA-Zn prepared in Example 1, Example 2, Example 3 and Comparative Example 1 II @Energy storage density and energy storage efficiency of SiO2 / PEI composite film and PEI film at 25℃ and 150℃. As can be seen from the figure, when the doping amount is 0.3%, TA-Zn II @SiO2 / PEI composite film has an electric field strength of 5.9J / cm at 600kV / mm 3 The energy storage density is 85.6%, which is 3.37 J / cm2 higher than that of pure PEI film. 3 Although the 0.1% composite film has 6.2J / cm 3 The energy storage density of the composite film is 3.2 J / cm2 at an electric field strength of 420 kV / mm. 3 The energy storage density of the composite film was improved, and the energy storage efficiency was increased to 87.3%. This result shows that a higher doping content is not conducive to improving the energy storage density of the polymer dielectric. At high temperature of 150°C, the component with the best energy storage performance of the composite film is still 0.3wt%, which has an energy storage efficiency of 4.8J / cm at an electric field strength of 620kV / mm.3 The energy storage density of the polymer dielectric decreased, and the energy storage efficiency dropped to 81.8%. It can be seen that the energy storage density and energy storage efficiency of the polymer dielectric will decrease with the increase of temperature, but the presence of the SiO2 core layer and the tannic acid metal organic framework shell layer improves the energy storage performance of the polymer dielectric.

Claims

1. A method for preparing a modified polyetherimide-based composite dielectric film, characterized in that: The following steps are involved: Step 1, dissolving 0.02-0.06 g of tannic acid in 25-75 mL of deionized water to prepare a tannic acid solution, dissolving 0.005-0.015 g of zinc sulfate heptahydrate in 25-75 mL of deionized water to prepare a zinc sulfate heptahydrate solution, and dissolving 0.05-0.15 g of hydroxyl-modified silica nanoparticles in 50-150 mL of deionized water to prepare a silica dispersion; Step 2, adding the zinc sulfate solution to the silicon dioxide dispersion prepared in step 1 and mixing them evenly to obtain a zinc sulfate silicon dioxide mixed solution, then adding the tannic acid solution to the zinc sulfate silicon dioxide mixed solution and mixing them evenly, centrifuging and washing them multiple times at a speed of 12000 rpm, and freeze-drying to prepare a core-shell structure filler TA-Zn II @SiO2; Step 3: Dissolve 1.5-4.5 g of 4,4'-diaminodiphenyl ether required for polyetherimide in 18.3-54.9 mL of N-methyl-2-pyrrolidone solvent to obtain a diamine dispersion; then II @Add SiO2 filler into diamine dispersion and stir evenly; Step 4, weighing 4.019-12.057 g of bisphenol A diether dianhydride, and adding it to the diamine dispersion in 6 portions to obtain a polyamic acid colloid; Step 5, vacuum bubble the polyamic acid colloid, then use a scraper to evenly coat the polyamic acid colloid on a glass plate, and then place it in a high-temperature oven to remove the solvent in the film, keep it warm at 150°C for 1 hour, 200°C for 1 hour, 250°C for 1 hour, and 300°C for 1 hour, and after natural cooling, obtain a modified polyetherimide-based composite dielectric film.

2. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In the step 1, the concentration of the tannic acid solution is 0.0004-0.0012 mol / L, and the concentration of the zinc sulfate heptahydrate solution is 0.0012-0.0036 mol / L.

3. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In the step 2, when the tannic acid solution is mixed with the zinc sulfate-silicon dioxide mixed solution, it is necessary to carry out the process under ultrasonic conditions, and the ultrasonic time is 8-10s.

4. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In the step 3, 4,4'-diaminodiphenyl ether is dispersed in N-methyl-2-pyrrolidone solvent by ultrasonication for 5-15 minutes.

5. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In step 3, adding core-shell structure filler TA-Zn II @The mass of SiO2 filler is 0.1%-0.5% of the total mass of 4,4'-diaminodiphenyl ether and bisphenol A diether dianhydride.

6. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In the step 4, bisphenol A diether dianhydride is added to the diamine dispersion, and the addition amounts for 6 times are 2-6g, 1-3g, 0.5-1.5g, 0.3-0.9g, 0.1-0.3g, and 0.119-0.357g, respectively, and the stirring time after each addition is 10-20min, 10-20min, 10-20min, 10-20min, 20-40min, and 60-120min, respectively.

7. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In the step 4, during the addition of bisphenol A diether dianhydride, the temperature is kept at 0-10°C and the mechanical stirring speed is 3000 rpm.

8. The method for preparing a modified polyetherimide-based composite dielectric film according to claim 1, characterized in that: In the step 5, the temperature and time for removing the solvent in the film are 80-90° C. and 12-18 h respectively.

Citation Information

Patent Citations

  • Preparation method of low-dielectric all-organic polyimide composite film for electronic packaging

    CN116925399A

  • Polyimide mixed matrix membrane as well as preparation method and application thereof

    CN117018896A

  • Preparation method of polyetherimide-based nano composite material for energy storage dielectric

    CN117362721A

  • Modified polyimide material as well as preparation method and application thereof

    CN118048039A

  • High-energy-storage polyetherimide dielectric material as well as preparation method and application thereof

    CN118126322A