High-dielectric high-temperature-resistant polyetherimide dielectric film as well as preparation method and application thereof

By introducing fluorene and ether bonds into the polyetherimide dielectric film, binding hydroxyl groups, and regulating the imidation reaction, the problems of low dielectric constant and poor temperature resistance in the prior art are solved, and high dielectric is achieved The improvement of constant and high temperature resistance significantly improves insulation performance and energy storage efficiency.

CN118930858APending Publication Date: 2024-11-12ELECTRIC POWER RES INST CHINA SOUTHERN POWER GRID CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411263043.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polymer capacitor film has a low dielectric constant and poor temperature resistance, which cannot meet the needs of new energy vehicles and electromagnetic catapults in extreme environments.

Method used

High dielectric high-temperature resistant polyetherimide dielectric film is adopted. The main chain of the molecule contains fluorene and ether bonds and the side chain contains hydroxyl groups. By regulating the imidation temperature, the reaction process is controlled, and a small amount of incompletely reacted diamine monomers are used. The body uses carriers to capture traps, suppress conductivity loss and improve insulation performance.

Benefits of technology

The dielectric constant, glass transition temperature and temperature resistance of the material are significantly improved, the insulation performance and energy storage efficiency are enhanced, and the material exhibits good flexibility and mechanical strength at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930858A_ABST
    Figure CN118930858A_ABST
Patent Text Reader

Abstract

The invention discloses a high-dielectric high-temperature-resistant polyetherimide dielectric film and a preparation method and application thereof, and belongs to the technical field of polymer film capacitor materials. The invention aims to solve the bottleneck problems of low dielectric constant and poor temperature resistance of the existing polymer capacitor film. According to the invention, 4, 4-(4, 4-isopropyl diphenoxy) bis (phthalic anhydride), 9, 9-bis (3-amino-4-hydroxyphenyl) fluorene and 4, 4 '-diaminodiphenyl ether are fully dissolved in an organic solvent, and the colloid is further prepared by adopting a solution tape casting method and a gradient heating imidization reaction. The energy storage density of the prepared high-dielectric high-temperature-resistant polyetherimide dielectric film reaches 3.88 J / cm < 3 > when the charging and discharging efficiency is greater than 90% at 150 DEG C. In addition, the used preparation process is simple and convenient to operate, green and environment-friendly, and can be popularized and used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer film capacitor materials, and in particular relates to a high-dielectric, high-temperature-resistant polyetherimide dielectric film and a preparation method and application thereof. Background Art

[0002] Dielectric capacitors have ultra-high power density of megawatts and excellent discharge rates of microseconds, and have become an important component of electronic devices and power equipment. Polymer dielectric films are often used as energy storage materials in capacitors due to their excellent electrical insulation properties, easy processing, and low cost. As electrical equipment develops towards high thermal stability, large capacity, and high integration, film capacitors and their key insulating materials face severe challenges. The development of temperature-resistant and high-energy storage density energy storage media has become a research hotspot in the field of electrical materials.

[0003] Biaxially oriented polypropylene (BOPP) is currently the most successful commercial dielectric film capacitor material, with advantages such as excellent insulation strength and low dielectric loss. However, the dielectric constant and long-term permissible temperature of BOPP are low, which cannot meet the service requirements in extreme environments such as new energy vehicles, electromagnetic catapults, and oil and gas extraction. Therefore, it is crucial to develop a dielectric film with high dielectric constant and good temperature resistance. Summary of the invention

[0004] The purpose of the present invention is to solve the bottleneck problem of low dielectric constant and poor temperature resistance of existing polymer capacitor films, and to provide a high dielectric and high temperature resistant polyetherimide dielectric film and its preparation method and application.

[0005] A high-dielectric and high-temperature resistant polyetherimide dielectric film has a main molecular chain containing fluorene and ether bonds and a side chain containing hydroxyl groups; the high-dielectric and high-temperature resistant polyetherimide dielectric film has a glass transition temperature of 251.25°C to 287.47°C, a dielectric constant of 3.35 to 3.55, a breakdown field strength of 529.1 MV / m to 652.2 MV / m, and a discharge energy density of 3.75 J / cm at 150°C 3 ~6.54J / cm 3 The charge and discharge efficiency is 65.31% to 82.29%.

[0006] The present invention controls the imidization reaction process by regulating the imidization temperature, and a small amount of incompletely reacted diamine monomers act as carrier capture traps to suppress conductivity loss and improve insulation performance. The hydroxyl group and the fluorene benzene ring structure increase the dielectric constant and glass transition temperature of the film, while the ether bond maintains the excellent flexibility of the polymer film.

[0007] A method for preparing a high-dielectric, high-temperature-resistant polyetherimide dielectric film is specifically completed by the following steps:

[0008] 1. Place 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in a vacuum drying oven and let stand for a period of time for later use;

[0009] 2. Under vacuum, dissolving 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in an organic solvent to obtain a mixed solution I;

[0010] 3. gradually adding 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride) into the mixed solution I, and stirring under vacuum until completely dissolved to obtain a polyetheramic acid precursor solution;

[0011] Fourth, the polyetheramic acid precursor solution is cast onto a clean glass substrate by a solution casting method, and then the temperature is gradually increased for thermal imidization to obtain a high-dielectric and high-temperature resistant polyetherimide dielectric film.

[0012] A high-dielectric and high-temperature resistant polyetherimide dielectric film is used for preparing polymer film capacitors.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. The preparation process of the present invention is simple, and the reactions are all carried out in the liquid phase, which can realize large-scale coating and is well compatible with the "roll-to-roll" preparation process of industrial capacitor film production;

[0015] 2. The polyetherimide film material prepared by the present invention introduces hydroxyl groups, which significantly improves the dielectric properties of the material. The benzene ring structure of fluorene increases the glass transition temperature of the material and improves the heat resistance. At the same time, the ether bond of the novel polyetherimide molecular structure enables the film to maintain mechanical strength while having good processing performance and flexibility;

[0016] 3. The present invention regulates the progress of the imidization reaction by changing the thermal imidization temperature. A small amount of diamine monomer that has not completely reacted can serve as a carrier capture trap, effectively suppressing conduction loss at high temperature, thereby improving the insulation performance and energy storage efficiency of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 The chemical structural formulas of the synthetic monomers used in the present invention are 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, and 4,4'-diaminodiphenyl ether;

[0018] Figure 2 This is a SEM image of the high-dielectric and high-temperature-resistant polyetherimide dielectric film prepared in Example 2;

[0019] Figure 3 XRD patterns of high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3;

[0020] Figure 4 Fourier transform infrared spectra of the high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3;

[0021] Figure 5 DSC curves of high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3;

[0022] Figure 6 The dielectric spectrum of the high dielectric and high temperature resistant polyetherimide dielectric film prepared in Examples 1 to 3 at 150°C;

[0023] Figure 7 The high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3 were 3 Dielectric temperature spectrum at Hz;

[0024] Figure 8 The Weibull breakdown strength distribution diagram of the high dielectric and high temperature resistant polyetherimide dielectric film prepared in Examples 1 to 3 at 150° C.;

[0025] Fig. 9 This is a graph showing the energy storage characteristics of the high-dielectric and high-temperature-resistant polyetherimide dielectric film prepared in Examples 1 to 3 as a function of the electric field intensity at 150°C. DETAILED DESCRIPTION

[0026] Specific implementation method 1: This implementation method is a high dielectric and high temperature resistant polyetherimide dielectric thin film, the main chain of which contains fluorene and ether bonds, and the side chain contains hydroxyl groups; the high dielectric and high temperature resistant polyetherimide dielectric film has a glass transition temperature of 251.25°C to 287.47°C, a dielectric constant of 3.35 to 3.55, a breakdown field strength of 529.1MV / m to 652.2MV / m, and a discharge energy density of 3.75J / cm at 150°C. 3 ~6.54J / cm 3 The charge and discharge efficiency is 65.31% to 82.29%.

[0027] Specific implementation method 2: This implementation method is a method for preparing a high-dielectric, high-temperature-resistant polyetherimide dielectric film, which is specifically completed in the following steps:

[0028] 1. Place 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in a vacuum drying oven and let stand for a period of time for later use;

[0029] 2. Under vacuum, dissolving 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in an organic solvent to obtain a mixed solution I;

[0030] 3. gradually adding 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride) into the mixed solution I, and stirring under vacuum until completely dissolved to obtain a polyetheramic acid precursor solution;

[0031] Fourth, the polyetheramic acid precursor solution is cast onto a clean glass substrate by a solution casting method, and then the temperature is gradually increased for thermal imidization to obtain a high-dielectric and high-temperature resistant polyetherimide dielectric film.

[0032] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the molar ratio of 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, 4,4'-diaminodiphenyl ether and 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride) described in step 1 is 0.5:0.5:1.05. The other steps are the same as those of specific embodiment 1 or 2.

[0033] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the temperature of the vacuum drying oven in step 1 is 70°C to 90°C and the standing time is 8h to 10h. The other steps are the same as those in specific embodiments 1 to 3.

[0034] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the organic solvent in step 2 is N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone. The other steps are the same as those in specific embodiments 1 to 4.

[0035] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the reaction temperature in step 3 is room temperature and the stirring time is 10 h to 12 h. The other steps are the same as those of specific embodiments 1 to 5.

[0036] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the solid content of the polyetheramic acid precursor solution in step 3 is 15% to 20%. The other steps are the same as those of specific embodiments 1 to 6.

[0037] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that: the specific process of thermal imidization described in step four is: gradient heating is adopted, the heating rate is 5°C / min to 10°C / min, the temperature interval of the gradient heating is 25°C to 50°C, each temperature is kept constant for 60min to 90min, and the final temperature of thermal imidization is 250°C to 350°C. The other steps are the same as those of specific embodiments one to seven.

[0038] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: after the thermal imidization in step 4, the glass substrate needs to be soaked in deionized water for 6h to 8h for peeling, and the peeled film needs to be placed in a vacuum oven at 100℃ to 110℃ for 10h to 12h; the thickness of the high-dielectric and high-temperature resistant polyetherimide dielectric film is 5μm to 15μm. The other steps are the same as those of specific embodiments 1 to 8.

[0039] Specific embodiment 10: This embodiment is a high-dielectric and high-temperature resistant polyetherimide dielectric film used to prepare a polymer film capacitor. The other steps are the same as those of specific embodiments 1 to 9.

[0040] The following examples are used to verify the beneficial effects of the present invention:

[0041] Embodiment 1: A method for preparing a high-dielectric and high-temperature resistant polyetherimide dielectric film is specifically completed by the following steps:

[0042] 1. Place 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in a vacuum drying oven at 80°C for 9 hours for later use;

[0043] 2. Under vacuum, 1.7551 g of 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 1.1563 g of 4,4'-diaminodiphenyl ether were dissolved in 30.0 mL of N,N-dimethylacetamide to obtain a mixed solution I;

[0044] 3. 5.5717 g of 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride) was added to the mixed solution I in batches, and stirred for 12 hours at room temperature and vacuum environment to obtain a polyetheramic acid precursor solution;

[0045] The solid content of the polyetheramic acid precursor solution described in step 3 is 15%;

[0046] Fourth, the polyetheramic acid precursor solution was placed in a vacuum oven at room temperature for 12 hours with a vacuum degree of -0.1 MPa to expel bubbles in the colloid to obtain a colloid with bubbles expelled;

[0047] 5. Slowly pour the colloid with bubbles discharged onto a clean and dry glass substrate, and use a scraper to evenly coat the colloid on the glass substrate; place the glass substrate in a constant temperature oven at 80°C for 12 hours to volatilize most of the solvent;

[0048] 6. Transfer the glass substrate in step 5 to a high-temperature blast oven for thermal imidization reaction; the thermal imidization process adopts a gradient heating method, the heating rate is 5°C / min, and the gradient heating program is set as follows: 80°C→100°C→150°C→200°C→250°C, and keep constant at 80°C, 100°C, 150°C, 200°C and 250°C for 60 minutes respectively;

[0049] 7. After the oven is cooled to room temperature naturally, the glass substrate is soaked in deionized water and peeled for 6 hours. The peeled film needs to be placed in a vacuum oven at 100°C for 12 hours;

[0050] The thickness of the high-dielectric and high-temperature-resistant polyetherimide dielectric film described in step seven is 10 μm.

[0051] Example 2: The difference between this example and Example 1 is that in step 6, the glass substrate in step 5 is transferred to a high-temperature blast oven for thermal imidization reaction; the thermal imidization process adopts a gradient heating method, the heating rate is 5°C / min, and the gradient heating program is set as follows: 80°C→100°C→150°C→200°C→250°C→300°C, and the temperatures at 80°C, 100°C, 150°C, 200°C, 250°C and 300°C are kept constant for 60 minutes respectively. The other steps and parameters are the same as those in Example 1.

[0052] The thickness of the high-dielectric and high-temperature-resistant polyetherimide dielectric film prepared in Example 2 is 10 μm.

[0053] Example 3: The difference between this example and Example 1 is that in step 6, the glass substrate in step 5 is transferred to a high-temperature blast oven for thermal imidization reaction; the thermal imidization process adopts a gradient heating method, the heating rate is 5°C / min, and the gradient heating program is set as follows: 80°C→100°C→150°C→200°C→250°C→300°C→350°C, and the temperatures are kept constant at 80°C, 100°C, 150°C, 200°C, 250°C, 300°C and 350°C for 60 minutes respectively. The other steps and parameters are the same as those in Example 1.

[0054] Figure 2 This is a SEM image of the high-dielectric and high-temperature-resistant polyetherimide dielectric film prepared in Example 2;

[0055] from Figure 2It can be seen that the cross-sectional structure of the film is dense and smooth, without obvious defects such as holes and cracks.

[0056] Figure 3 XRD patterns of high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3;

[0057] from Figure 3 It can be seen that the high-dielectric and high-temperature-resistant polyetherimide dielectric films prepared in Examples 1 to 3 are all of amorphous structures.

[0058] Figure 4 Fourier transform infrared spectra of the high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3;

[0059] Figure 4 The high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3 show the high dielectric constant at 3430 cm -1 The presence of the stretching vibration peak of -OH at proves the successful introduction of hydroxyl group.

[0060] Figure 5 DSC curves of high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3;

[0061] Figure 5 The glass transition temperatures of the high-dielectric and high-temperature-resistant polyetherimide dielectric films prepared in Examples 1 to 3 are 251.25° C., 263.3° C., and 287.47° C., respectively, which are significantly higher than the glass transition temperature (217° C.) of the currently commercially available Ultem 1000 polyetherimide.

[0062] Figure 6 The dielectric spectrum of the high dielectric and high temperature resistant polyetherimide dielectric film prepared in Examples 1 to 3 at 150°C;

[0063] Figure 7 The high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3 were 3 Dielectric temperature spectrum at Hz;

[0064] Figure 6 , 7 The high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3 have good thermal conductivity at 150°C and 10 3 The dielectric constants at Hz are 3.55, 3.41, and 3.35 respectively; the dielectric constants of the currently commercially available Ultem 1000 polyetherimide are 3.03.

[0065] Figure 8The Weibull breakdown strength distribution diagram of the high dielectric and high temperature resistant polyetherimide dielectric film prepared in Examples 1 to 3 at 150° C.;

[0066] Figure 8 It shows that the characteristic breakdown field strengths of the high dielectric and high temperature resistant polyetherimide dielectric films prepared in Examples 1 to 3 at 150°C are 576.7 MV / m, 652.2 MV / m, and 529.1 MV / m, respectively; the characteristic breakdown field strength of the currently commercially available Ultem 1000 polyetherimide is 494.4 MV / m.

[0067] Fig. 9 The energy storage characteristics of the high dielectric and high temperature resistant polyetherimide dielectric film prepared in Examples 1 to 3 vary with the electric field strength at 150°C;

[0068] Fig. 9 The high dielectric and high temperature resistant polyetherimide dielectric film prepared in Example 2 has a discharge energy density of 6.54 J / cm at 150°C. 3 At this time, the charge and discharge efficiency is 82.29%; when the charge and discharge efficiency is greater than 90%, the discharge energy density is 3.88J / cm 3 , which is 2.34J / cm2 under the same conditions as the currently available Ultem 1000 polyetherimide. 3 Significantly improved compared to the previous study.

[0069] Compared with the prior art, the present invention selects diamine monomers with different functional groups and adopts a two-step method to synthesize a modified polyetherimide-based capacitor film, which is easy to prepare. By changing the temperature of thermal imidization to control the reaction process, a small amount of incompletely reacted diamine monomers can be used as carrier capture traps to suppress conduction losses. At the same time, hydroxyl, fluorene, and ether bond functional groups are introduced into the molecular chain to significantly improve the relative dielectric constant and glass transition temperature of the modified film while maintaining the flexibility of the polymer film. The modified polymer film prepared by the present invention has an energy storage density of 3.88 J / cm at 150°C and a charge and discharge efficiency of >90%. 3 , and the breakdown strength, dielectric properties, thermal stability, etc. have been improved, and the energy storage characteristics are good.

Claims

1. A high dielectric and high temperature resistant polyetherimide dielectric film, Features The high-dielectric and high-temperature-resistant polyetherimide dielectric film has fluorene and ether bonds in the main molecular chain and hydroxyl groups in the side chain; the high-dielectric and high-temperature-resistant polyetherimide dielectric film has a glass transition temperature of 251.25° C. to 287.47° C., a dielectric constant of 3.35 to 3.55, a breakdown field strength of 529.1 MV / m to 652.2 MV / m, and a discharge energy density of 3.75 J / cm at 150° C. 3 ~6.54J / cm 3 The charge and discharge efficiency is 65.31% to 82.29%.

2. A method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film as claimed in claim 1, Features The preparation method is specifically completed according to the following steps:

1. Place 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in a vacuum drying oven and let stand for a period of time for later use; 2. Under vacuum, dissolving 9,9-bis(3-amino-4-hydroxyphenyl)fluorene and 4,4'-diaminodiphenyl ether in an organic solvent to obtain a mixed solution I; 3. gradually adding 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride) into the mixed solution I, and stirring under vacuum until completely dissolved to obtain a polyetheramic acid precursor solution; Fourth, the polyetheramic acid precursor solution is cast onto a clean glass substrate by a solution casting method, and then the temperature is gradually increased for thermal imidization to obtain a high-dielectric and high-temperature resistant polyetherimide dielectric film.

3. A method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features The molar ratio of 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, 4,4'-diaminodiphenyl ether and 4,4-(4,4-isopropyldiphenoxy)bis(phthalic anhydride) in step 1 is 0.5:0.5:1.

05.

4. The method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features The temperature of the vacuum drying oven described in step 1 is 70° C. to 90° C.; the standing time described is 8 h to 10 h.

5. The method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features The organic solvent described in step 2 is N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.

6. The method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features The reaction temperature in step 3 is room temperature, and the stirring time is 10 h to 12 h.

7. The method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features The solid content of the polyetheramic acid precursor solution described in step 3 is 15% to 20%.

8. The method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features The specific process of thermal imidization described in step 4 is: using gradient heating, the heating rate is 5°C / min~10°C / min, the temperature interval of the gradient heating is 25°C~50°C, each temperature is kept constant for 60min~90min, and the final temperature of thermal imidization is 250°C~350°C.

9. The method for preparing a high dielectric and high temperature resistant polyetherimide dielectric film according to claim 2, Features After the thermal imidization in step 4 is completed, the glass substrate needs to be immersed in deionized water for 6h to 8h for peeling, and the peeled film needs to be placed in a vacuum oven at 100°C to 110°C for 10h to 12h; the thickness of the high-dielectric and high-temperature resistant polyetherimide dielectric film is 5μm to 15μm.