Preparation method of modified organic silicon resin for LED packaging
The modified silicone resin process of grafting polymerization and introducing titanium through one-pot method has solved the problem of refractive index mismatch of LED packaging materials, improved temperature resistance and light transmittance, and is suitable for high-temperature LED packaging.
Patent Information
- Application Number
- CN202411182180.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
The existing low-refractive index silicone materials used in LED packaging have total reflection of light due to refractive index mismatch, which reduces the light extraction efficiency. At the same time, their preparation process efficiency is low and their temperature resistance is insufficient.
The graft polymerization of the modified silicone resin is carried out by a one-pot method, and titanium is introduced into the reaction system, and the modified silicone resin containing titanium is formed by curing ultraviolet light to improve the temperature resistance and light transmittance of the resin.
It improves reaction efficiency, reduces production costs, significantly improves the temperature resistance and light transmittance of the resin, and is suitable for high-temperature LED packaging applications.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic silicon resin materials, and more specifically to a preparation method of modified organic silicon resin for LED packaging. Background Art
[0002] LED, the full name of light-emitting diode, is a semiconductor element that can convert electrical energy into light energy. It is mainly composed of compounds containing gallium, arsenic, phosphorus, nitrogen and other elements. Its core component is a semiconductor chip. By adjusting the material composition of the chip, it can achieve the emission of visible light of different wavelengths, thereby producing a variety of color light. The basic characteristics of LED make it an ideal choice to replace traditional light sources. It has been widely used in fields such as indication, signal and landscape lighting. According to the different packaging and structural types of LED products, appropriate packaging solutions need to be designed. Only packaged LEDs can be transformed into actual products and put on the market. Therefore, for light-emitting diodes (LEDs), the packaging process plays a vital role.
[0003] With the continuous expansion of LED applications, the requirements for its packaging materials are becoming increasingly stringent. At present, the main packaging materials used for LEDs include epoxy resins and silicone materials. Epoxy resins are known for their high strength and good substrate adhesion. However, their defects such as excessive internal stress, insufficient UV resistance, poor high temperature resistance, weak aging resistance, and excessive light decay after lighting limit their application. In contrast, low-refractive-index silicone materials exhibit superior comprehensive properties, including less internal stress, excellent high and low temperature tolerance, excellent high-temperature yellowing resistance and UV resistance, and lower light decay after long-term lighting. Therefore, silicone materials quickly replaced epoxy resins and have been widely used in the field of LED packaging. However, due to the large difference between the low-refractive-index silicone materials (refractive index of 1.40) used for LED packaging and the chip refractive index (2.4), this refractive index mismatch will lead to total reflection, causing the light to be reflected back into the chip and cannot be effectively exported, thereby reducing the light extraction efficiency.
[0004] Chinese Patent Publication No. CN105399956A discloses a high-temperature resistant, high-refractive-index titanium-containing silicone resin and a preparation method thereof, which provides a titanium-containing silicone resin. In fact, the LED is bonded by additionally adding a silicone coupling agent, but the silicone coupling agent has a poor bonding effect; Chinese Patent Publication No. CN112760079A discloses a high-refractive silicone packaging material and a preparation method thereof, which provides a platinum-added silicone packaging material for LEDs, but elements such as N, P, and S are prone to platinum poisoning and poor curing; Chinese Patent Publication No. CN117024706A discloses a UV-curable modified silicone resin and a preparation method thereof, which provides a UV-curable modified silicone resin. The process is to synthesize the resin by an intermittent reaction grafting method. This synthesis method requires multiple batches to produce the resin, resulting in low production efficiency and difficulty in ensuring consistency between batches. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the present invention provides a method for preparing a modified silicone resin for LED encapsulation, which adopts a one-pot method to graft polymerize the modified silicone resin to improve the reaction efficiency, and introduces titanium to improve the temperature resistance of the resin.
[0006] The technical solution of the present invention is as follows: A method for preparing a modified silicone resin for LED packaging, comprising the following steps:
[0007] (1) Preparation of modified silicone resin prepolymer: hydrolyze polyethyl silicate, then add alcohol, ketone or ester solvent, deionized water, epoxysiloxane and diisocyanate to the hydrolyzate, then add the pre-mixed polyether diol, phenylsiloxane and end-capping agent mixture to the above reaction system in a dropwise manner to obtain a modified silicone resin prepolymer;
[0008] (2) Preparation of titanium-modified silicone resin prepolymer: under nitrogen protection, titanate is slowly added dropwise to the modified silicone resin prepolymer to generate a light yellow transparent liquid; the light yellow transparent liquid is subjected to a reduced pressure and temperature treatment to remove the solvent and small molecular impurities to obtain a titanium-containing modified silicone resin prepolymer;
[0009] (3) UV curing: The titanium-containing modified silicone resin prepolymer and the photoinitiator are mixed in proportion and stirred evenly, and then the evenly stirred mixture is degassed. The degassed mixture can be photocured under ultraviolet light to form a titanium-containing modified silicone resin cured product.
[0010] Preferably, in step (1), the preparation process of the modified silicone resin prepolymer is as follows:
[0011] a. Hydrolyze polyethyl silicate under acidic or alkaline conditions at 0-10°C for 0.5-1h;
[0012] b. Add alcohol, ketone or ester solvent, deionized water, epoxysiloxane and diisocyanate to the hydrolyzate obtained in step a, maintain the temperature of the reaction system between 10° C. and 20° C., and continue stirring the reaction for 0.5 h to 1 h;
[0013] c. Add the pre-mixed polyether diol, phenylsiloxane and end-capping agent mixture dropwise to the reaction system obtained in step b within 10 to 30 minutes, then heat the reaction system to 70 to 100° C. and keep the reaction within this temperature range for 3 to 6 hours to complete the grafting and polymerization reaction;
[0014] d. After the reaction is completed, the reaction mixture is cooled to room temperature and subjected to extraction and separation using an aromatic solvent. The lower layer of liquid after the extraction and separation is taken and subjected to neutralization and water removal treatment to obtain a modified silicone resin prepolymer.
[0015] Preferably, in step (2), the preparation process of the titanium-modified silicone resin prepolymer is as follows:
[0016] e. Under nitrogen protection, the modified silicone resin prepolymer prepared in step d is placed in a reaction container, and titanate is slowly added thereto; the temperature of the reaction system is controlled at 60° C., and the temperature is maintained for 6 hours, during which nitrogen is continuously introduced to maintain an inert atmosphere, and the reaction generates a light yellow transparent liquid;
[0017] f. The light yellow transparent liquid obtained in step e is subjected to a reduced pressure and temperature treatment, and desolventizing and small molecule reaction are carried out at 150° C. and a pressure of 0.09 MPa to remove unreacted titanate, solvent and other small molecule impurities to obtain a modified silicone resin prepolymer containing titanium.
[0018] Preferably, the ingredients of the modified silicone resin prepolymer are fed in the following proportions:
[0019] 2-3 parts of acidic or alkaline catalyst; 100-150 parts of polyethyl silicate; 10-20 parts of alcohol / ketone / ester solvent; 10-20 parts of deionized water; 10-20 parts of epoxysiloxane; 20-40 parts of diisocyanate; 20-40 parts of polyether diol; 10-30 parts of phenylsiloxane; 20-40 parts of end-capping agent; 40-50 parts of xylene.
[0020] Preferably, the polyether diol is selected from one or more of PEG200, PEG400, PEG600, PEG800, PEG1000, PEG5000, and PEG10000.
[0021] Preferably, the diisocyanate is one or more of toluene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate, and hexamethylene diisocyanate.
[0022] Preferably, the catalyst comprises an acidic catalyst or a basic catalyst, the acidic catalyst comprises hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, phosphorous acid, hypophosphorous acid, iodic acid or superphosphoric acid; the basic catalyst comprises sodium hydroxide, potassium hydroxide, aluminum hydroxide, sodium bicarbonate, ammonium bicarbonate, sodium carbonate or tetramethylammonium hydroxide.
[0023] Preferably, the capping agent has the structure (CH3)2R1SiOSiR2(CH3)2, wherein R1 and R2 are CH3 and phenyl, respectively.
[0024] Preferably, the titanate is one or more of tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, n-butyl titanate, tetraisobutyl titanate, di(acetylacetonato)diisopropyl titanate, isopropoxy tri(dioctyl phosphate) titanate, isopropyl trioleyl titanate, and isopropyl triisostearate titanate; the added amount of the titanate is 0.5-1% of the total amount of the modified silicone resin prepolymer.
[0025] Preferably, the photoinitiator is one or more of xanthenyl phenyl iodonium salt, fluorenyl phenyl iodonium salt, isopropylbenzene (II) hexafluorophosphate, dialkylbenzoyl sulfonium salt, triaryl (1-pyrene) bismuthium salt, dialkylbenzoyl sulfonium salt, dialkylbenzoyl sulfonium salt, bis(5-fluorothiophene-2-yl) iodonium formate, S,S-dialkyl-S-(dimethylhydroxyphenyl) sulfonium salt and phenylthiophenyl diphenyl sulfonium salt; the added amount of the photoinitiator is 1 to 3% of the total amount of the titanium-containing modified silicone resin prepolymer.
[0026] The present invention according to the above scheme has the following beneficial effects:
[0027] (1) The present invention provides a method for preparing a modified silicone resin for LED encapsulation. By adopting a "one-pot method" to carry out graft polymerization of the modified silicone resin, all necessary reactants and catalysts are added to the reaction system at one time, avoiding the separation and purification steps of the intermediate products. This continuous reaction process significantly improves the reaction efficiency, shortens the preparation cycle, and reduces the production cost. At the same time, the one-pot method promotes sufficient contact and mixing between the reactants, which is conducive to the rapid reaction and uniform generation of the product.
[0028] (2) The present invention provides a method for preparing a modified silicone resin for LED encapsulation, which introduces titanate into the reaction system and reacts under nitrogen protection to prepare a modified silicone resin prepolymer containing titanium; the addition of titanium significantly improves the heat resistance of the resin and can effectively resist the damage of high temperature to the resin structure; this improvement in heat resistance makes the modified silicone resin have a wider range of use prospects in high-temperature applications such as LED encapsulation. Secondly, the introduction of organic titanium not only improves the heat resistance of the resin, but also improves its light transmittance because the titanium compound forms a microstructure in the resin that is conducive to light transmission. DETAILED DESCRIPTION
[0029] The following embodiments of the present invention are further described in detail in conjunction with the examples. The detailed description of the following examples is used to illustrate the present invention, but cannot be used to limit the scope of the present invention, that is, the present invention is not limited to the described embodiments.
[0030] In order to better understand the present invention, the present invention is further described below in conjunction with the embodiments:
[0031] The present invention provides a method for preparing a modified silicone resin for LED packaging as follows:
[0032] a. Hydrolyze polyethyl silicate under acidic or alkaline conditions at 0-10°C for 0.5-1h;
[0033] b. Add alcohol, ketone or ester solvent, deionized water, epoxysiloxane and diisocyanate to the hydrolyzate obtained in step a, maintain the temperature of the reaction system between 10° C. and 20° C., and continue stirring the reaction for 0.5 h to 1 h;
[0034] c. Add the pre-mixed polyether diol, phenylsiloxane and end-capping agent mixture dropwise to the reaction system obtained in step b within 10 to 30 minutes, then heat the reaction system to 70 to 100° C. and keep the reaction within this temperature range for 3 to 6 hours to complete the grafting and polymerization reaction;
[0035] d. After the reaction is completed, the reaction mixture is cooled to room temperature, and an aromatic solvent is used for extraction and separation. The lower layer of liquid after the extraction and separation is taken, and a modified silicone resin prepolymer is obtained after neutralization and dehydration.
[0036] e. Under nitrogen protection, titanate was slowly added dropwise to the modified silicone resin prepolymer, the temperature of the reaction system was controlled at 60° C., and the temperature was maintained for 6 hours, during which nitrogen was continuously introduced to maintain an inert atmosphere, and a light yellow transparent liquid was generated by the reaction;
[0037] f. subjecting the light yellow transparent liquid obtained in step e to a reduced pressure and temperature treatment, and performing a desolventizing and small molecule reaction at 150° C. and a pressure of 0.09 MPa to remove unreacted titanate, solvent and other small molecule impurities, thereby obtaining a modified silicone resin prepolymer containing titanium;
[0038] g. Mix the titanium-containing modified silicone resin prepolymer and the photoinitiator in proportion and stir them evenly, then degas the evenly stirred mixture, and the degassing mixture can be photocured under ultraviolet light to form a titanium-containing modified silicone resin cured product.
[0039] In the above steps a to d, the optimal ratio of each ingredient is added according to Table 1.
[0040] Table 1 Optimal ratio of ingredients
[0041] raw material Number of copies Acidic or basic catalyst 2~3 Ethyl Polysilicate 100~150 Alcohol / Ketone / Ester Solvents 10~20 Deionized water 10~20 Epoxy siloxane 10~20 Diisocyanates 20~40 Polyether diol 20~40 Phenyl siloxane 10~30 Capping agent 20~40 Xylene 40~50
[0042] Preferably, the alcohol solvent is one or more of methanol and ethanol.
[0043] Preferably, the ketone solvent is one or more of butanone, cyclohexanone and acetone.
[0044] Preferably, the polyether diol is preferably one or more of PEG200, PEG400, PEG600, PEG800, PEG1000, PEG5000, and PEG10000. (Polyether diol, also known as dihydroxy polyether, is an oligomer diol containing ether bond repeating units (-ROR-) in the molecule and having hydroxyl groups (-OH) at both ends. They are usually prepared by ring-opening polymerization of low molecular weight diols, polyamines and other low molecular weight compounds containing active hydrogen as initiators and compounds containing epoxy structures under the action of catalysts. Polyethylene glycol is a type of polyether diol, which is formed by connecting ethylene glycol monomers through ether bonds. PEG is widely used in the fields of medicine, cosmetics, food, etc.)
[0045] Preferably, the diisocyanate is one or more of the diisocyanates toluene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), naphthalene diisocyanate (XDI), and hexamethylene diisocyanate.
[0046] Preferably, the catalyst comprises an acidic catalyst or a basic catalyst, the acidic catalyst comprises hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, phosphorous acid, hypophosphorous acid, iodic acid or superphosphoric acid; the basic catalyst comprises sodium hydroxide, potassium hydroxide, aluminum hydroxide, sodium bicarbonate, ammonium bicarbonate, sodium carbonate or tetramethylammonium hydroxide.
[0047] Preferably, the capping agent is of the structure (CH3)2R1SiOSiR2(CH3)2; wherein R1 and R2 are CH3 and phenyl.
[0048] Preferably, the epoxy-containing siloxane is one or more of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane, 3-[(2,3)-epoxypropyloxy]propyltrimethoxysilane, 3-[(2,3)-epoxypropyloxy]propyltriethoxysilane, 2-(7-oxabicyclo[4.1.0]hept-3-yl)ethyltrimethoxysilane, 5,6-epoxyhexyltriethoxysilane, trimethoxy[2-(3,4-epoxycyclohexyl)methyldiethoxysilane 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane.
[0049] Preferably, the phenylsiloxane is one or more of 1,3-divinyl-1,3-dimethyl-1,3-diphenyldisiloxane, 1,1,3,3-tetramethyl-1,3-di-2-phenylethylated disiloxane, 1,3-dichlorotetraphenyldisiloxane, and 1,3-di(p-tolyl)-1,1,3,3-tetramethyldisiloxane.
[0050] Preferably, the silicate is one or more of methyl orthosilicate, ethyl orthosilicate, methyl polysilicate and ethyl polysilicate.
[0051] Preferably, the second solvent is one of xylene and hexamethyldisiloxane.
[0052] Preferably, the titanate is one or more of tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, n-butyl titanate, tetraisobutyl titanate, di(acetylacetonato)diisopropyl titanate, isopropoxy tri(dioctyl phosphate) titanate, isopropyl trioleyl titanate, triisostearate titanate isopropyl. The optimal addition amount is 0.5-1% of the total amount of the modified resin.
[0053] Preferably, the cationic photoinitiator is one or more of xanthenylphenyl iodonium salt, fluorenylphenyl iodonium salt, isopropylbenzene (II) hexafluorophosphate, dialkylbenzoyl sulfonium salt, triaryl (1-pyrene) bismuthium salt, dialkylbenzoyl sulfonium salt, dialkylbenzoyl sulfonium salt, bis (5-fluorothiophene-2-yl) iodonium formate, S, S-dialkyl-S- (dimethylhydroxyphenyl) sulfonium salt and phenylthiophenyl diphenyl sulfonium salt. The optimal addition amount is 1-3% of the total amount of the modified resin.
[0054] The specific embodiments are as follows
[0055] Example 1
[0056] (1) Preparation of modified silicone resin prepolymer
[0057] At 5°C, 100 parts of ethyl polysilicate were added to a reaction vessel, and 2 parts of tetramethylammonium hydroxide were added for hydrolysis, and the reaction was stirred for 0.5 hours; then 20 parts of butanone, 20 parts of deionized water, 10 parts of epoxysiloxane and 20 parts of diisocyanate were added to the hydrolyzate in sequence, while the temperature of the reaction system was kept at about 10°C, and stirring was continued for 1 hour to ensure sufficient mixing; within the next 30 minutes, 20 parts of PEG400 (polyethylene glycol 400), 10 parts of 1,1,3 ,3-tetramethyl-1,3-di-2-phenylethyl disiloxane and 20 parts of hexamethyldisiloxane are slowly added to the reaction system in a dropwise manner; after the dropwise addition is completed, the reaction system is heated to 90°C and the reaction is continued at this temperature for 6 hours; after the reaction is completed, the reaction system is allowed to cool naturally to room temperature or close to room temperature; then, xylene is used for extraction and separation to separate the lower layer of liquid, the lower layer of liquid is neutralized to remove residual alkaline substances, and water is removed by distillation or other methods to finally obtain a modified silicone resin prepolymer.
[0058] (2) Preparation of titanium-modified silicone resin prepolymer
[0059] Take 100 parts of the modified silicone resin prepolymer prepared in the above step (1), slowly add 1 part of titanate under nitrogen protection, and continue the reaction at 60°C for 6 hours, during which time the nitrogen atmosphere is maintained to prevent oxidation; after the reaction is completed, the reaction system is slowly reduced in pressure and heated to 150°C, and continued to be heated at a vacuum degree of 0.09 MPa to remove the solvent and small molecule impurities; when the solvent and small molecules are basically removed, a light yellow transparent titanium-containing modified silicone resin prepolymer is obtained.
[0060] (3) Preparation of UV-curable modified silicone resin
[0061] Take 50 parts of the titanium-containing modified silicone resin prepolymer prepared in the above step (2), add 1.5 parts of xanthenylphenyl iodonium salt as a photoinitiator; use a stirrer to fully stir the mixture to ensure that the photoinitiator is evenly dispersed in the resin; then degas the stirred mixture to remove bubbles generated during the mixing process to ensure that the surface of the cured product is smooth and defect-free; place the degassing mixture in an ultraviolet light curing device and perform light curing under ultraviolet light; finally, adjust the intensity and irradiation time of the ultraviolet light according to actual conditions until the mixture is completely cured to form a titanium-containing modified silicone resin cured product.
[0062] Example 2
[0063] (1) Preparation of modified silicone resin prepolymer
[0064] At 5°C, 100 parts of ethyl polysilicate were added to a reaction vessel, and 2 parts of tetramethylammonium hydroxide were added for hydrolysis, and the reaction was stirred for 0.5 hours. Then, 20 parts of butanone, 20 parts of deionized water, 10 parts of epoxysiloxane and 25 parts of diisocyanate were added to the hydrolyzate in sequence, while the temperature of the reaction system was kept at about 10°C, and stirring was continued for 1 hour to ensure sufficient mixing. In the next 30 minutes, 15 parts of PEG400 (polyethylene glycol 400), 10 parts of 1,1,3 ,3-tetramethyl-1,3-di-2-phenylethyl disiloxane and 20 parts of hexamethyldisiloxane are slowly added to the reaction system in a dropwise manner; after the dropwise addition is completed, the reaction system is heated to 90°C and the reaction is continued at this temperature for 6 hours; after the reaction is completed, the reaction system is allowed to cool naturally to room temperature or close to room temperature; then, xylene is used for extraction and separation to separate the lower layer of liquid, the lower layer of liquid is neutralized to remove residual alkaline substances, and water is removed by distillation or other methods to finally obtain a modified silicone resin prepolymer.
[0065] (2) Preparation of titanium-modified silicone resin prepolymer
[0066] Take 100 parts of the modified silicone resin prepolymer prepared in the above step (1), slowly add 1 part of titanate under nitrogen protection, and continue the reaction at 60°C for 6 hours, during which time the nitrogen atmosphere is maintained to prevent oxidation; after the reaction is completed, the reaction system is slowly reduced in pressure and heated to 150°C, and continued to be heated at a vacuum degree of 0.09 MPa to remove the solvent and small molecule impurities; when the solvent and small molecules are basically removed, a light yellow transparent titanium-containing modified silicone resin prepolymer is obtained.
[0067] (3) Preparation of UV-curable modified silicone resin
[0068] Take 50 parts of the titanium-containing modified silicone resin prepolymer prepared in the above step (2), add 1.5 parts of xanthenylphenyl iodonium salt as a photoinitiator; use a stirrer to fully stir the mixture to ensure that the photoinitiator is evenly dispersed in the resin; then degas the stirred mixture to remove bubbles generated during the mixing process to ensure that the surface of the cured product is smooth and defect-free; place the degassing mixture in an ultraviolet light curing device and perform light curing under ultraviolet light; finally, adjust the intensity and irradiation time of the ultraviolet light according to actual conditions until the mixture is completely cured to form a titanium-containing modified silicone resin cured product.
[0069] Example 3
[0070] (1) Preparation of modified silicone resin prepolymer
[0071] At 5°C, 100 parts of ethyl polysilicate were added to a reaction vessel, and 2 parts of tetramethylammonium hydroxide were added for hydrolysis, and the reaction was stirred for 0.5 hours; then 20 parts of butanone, 20 parts of deionized water, 10 parts of epoxysiloxane and 20 parts of diisocyanate were added to the hydrolyzate in sequence, while the temperature of the reaction system was kept at about 10°C, and stirring was continued for 1 hour to ensure sufficient mixing; within the next 30 minutes, 20 parts of PEG800 (polyethylene glycol 800) and 15 parts of 1,1,3 ,3-tetramethyl-1,3-di-2-phenylethyl disiloxane and 20 parts of hexamethyldisiloxane are slowly added to the reaction system in a dropwise manner; after the dropwise addition is completed, the reaction system is heated to 90°C and the reaction is continued at this temperature for 6 hours; after the reaction is completed, the reaction system is allowed to cool naturally to room temperature or close to room temperature; then, xylene is used for extraction and separation to separate the lower layer of liquid, the lower layer of liquid is neutralized to remove residual alkaline substances, and water is removed by distillation or other methods to finally obtain a modified silicone resin prepolymer.
[0072] (2) Preparation of titanium-modified silicone resin prepolymer
[0073] Take 100 parts of the modified silicone resin prepolymer prepared in the above step (1), slowly add 1 part of titanate under nitrogen protection, and continue the reaction at 60°C for 6 hours, during which time the nitrogen atmosphere is maintained to prevent oxidation; after the reaction is completed, the reaction system is slowly reduced in pressure and heated to 150°C, and continued to be heated at a vacuum degree of 0.09 MPa to remove the solvent and small molecule impurities; when the solvent and small molecules are basically removed, a light yellow transparent titanium-containing modified silicone resin prepolymer is obtained.
[0074] (3) Preparation of UV-curable modified silicone resin
[0075] Take 50 parts of the titanium-containing modified silicone resin prepolymer prepared in the above step (2), add 1.5 parts of xanthenylphenyl iodonium salt as a photoinitiator; use a stirrer to fully stir the mixture to ensure that the photoinitiator is evenly dispersed in the resin; then degas the stirred mixture to remove bubbles generated during the mixing process to ensure that the surface of the cured product is smooth and defect-free; place the degassing mixture in an ultraviolet light curing device and perform light curing under ultraviolet light; finally, adjust the intensity and irradiation time of the ultraviolet light according to actual conditions until the mixture is completely cured to form a titanium-containing modified silicone resin cured product.
[0076] Example 4
[0077] (1) Preparation of modified silicone resin prepolymer
[0078] At 5°C, 100 parts of ethyl polysilicate were added to a reaction vessel, and 2 parts of tetramethylammonium hydroxide were added for hydrolysis, and the reaction was stirred for 0.5 hours; then 20 parts of butanone, 20 parts of deionized water, 10 parts of epoxysiloxane and 20 parts of diisocyanate were added to the hydrolyzate in sequence, while the temperature of the reaction system was kept at about 10°C, and stirring was continued for 1 hour to ensure sufficient mixing; within the next 30 minutes, 20 parts of PEG800 (polyethylene glycol 800) and 20 parts of 1,1,3 ,3-tetramethyl-1,3-di-2-phenylethyl disiloxane and 20 parts of hexamethyldisiloxane are slowly added to the reaction system in a dropwise manner; after the dropwise addition is completed, the reaction system is heated to 90°C and the reaction is continued at this temperature for 6 hours; after the reaction is completed, the reaction system is allowed to cool naturally to room temperature or close to room temperature; then, xylene is used for extraction and separation to separate the lower layer of liquid, the lower layer of liquid is neutralized to remove residual alkaline substances, and water is removed by distillation or other methods to finally obtain a modified silicone resin prepolymer.
[0079] (2) Preparation of titanium-modified silicone resin prepolymer
[0080] Take 100 parts of the modified silicone resin prepolymer prepared in the above step (1), slowly add 1 part of titanate under nitrogen protection, and continue the reaction at 60°C for 6 hours, during which time the nitrogen atmosphere is maintained to prevent oxidation; after the reaction is completed, the reaction system is slowly reduced in pressure and heated to 150°C, and continued to be heated at a vacuum degree of 0.09 MPa to remove the solvent and small molecule impurities; when the solvent and small molecules are basically removed, a light yellow transparent titanium-containing modified silicone resin prepolymer is obtained.
[0081] (3) Preparation of UV-curable modified silicone resin
[0082] Take 50 parts of the titanium-containing modified silicone resin prepolymer prepared in the above step (2), add 1.5 parts of xanthenylphenyl iodonium salt as a photoinitiator; use a stirrer to fully stir the mixture to ensure that the photoinitiator is evenly dispersed in the resin; then degas the stirred mixture to remove bubbles generated during the mixing process to ensure that the surface of the cured product is smooth and defect-free; place the degassing mixture in an ultraviolet light curing device and perform light curing under ultraviolet light; finally, adjust the intensity and irradiation time of the ultraviolet light according to actual conditions until the mixture is completely cured to form a titanium-containing modified silicone resin cured product.
[0083] Comparative Example 1
[0084] (1) uniformly mixing one or more of α,ω-dihydroxy polydimethylsiloxane, tetraethyl orthosilicate, metal acid ester, and phenyl silicon diol to obtain a mixed solution;
[0085] (2) subjecting the mixed solution to atmospheric stirring, atmospheric distillation or reduced pressure distillation to obtain a modified silicone resin oligomer after completion, uniformly mixing the modified silicone resin oligomer with alkoxysilane to obtain a prepolymer mixed solution, and subjecting the prepolymer mixed solution to atmospheric distillation and / or reduced pressure distillation to obtain a modified silicone resin prepolymer;
[0086] (3) 50 parts of the modified silicone resin prepolymer prepared in the above step (2) and 1.5 parts of xanthenylphenyl iodonium salt were mixed and stirred evenly, and then degassed and cured under ultraviolet light.
[0087] Comparative Example 2
[0088] (1) Preparation of modified silicone resin prepolymer
[0089] At 5°C, 100 parts of ethyl polysilicate are added to a reaction container, and 2 parts of tetramethylammonium hydroxide are added for hydrolysis treatment, and the reaction is stirred for 0.5 hours; then 20 parts of butanone, 20 parts of deionized water and 10 parts of epoxysiloxane are added to the hydrolyzate in sequence, while the temperature of the reaction system is kept at about 10°C, and stirring is continued for 1 hour to ensure sufficient mixing; within the next 30 minutes, 10 parts of 1,1,3,3-tetramethyl-1,3-di-2-phenylethylated disiloxane and 20 parts of hexamethyldisiloxane that are pre-mixed uniformly are slowly added to the reaction system in a dropwise manner; after the dropwise addition is completed, the reaction system is heated to 90°C and the reaction is continued at this temperature for 6 hours; after the reaction is completed, the reaction system is allowed to cool naturally to room temperature or near room temperature; then xylene is used for extraction and separation to separate the lower layer of liquid, the lower layer of liquid is neutralized to remove residual alkaline substances, and water is removed by distillation or other methods to finally obtain a modified silicone resin prepolymer.
[0090] (2) Preparation of titanium-modified silicone resin prepolymer
[0091] Take 100 parts of the modified silicone resin prepolymer prepared in the above step (1), slowly add 1 part of titanate under nitrogen protection, and continue the reaction at 60°C for 6 hours, during which time the nitrogen atmosphere is maintained to prevent oxidation; after the reaction is completed, the reaction system is slowly reduced in pressure and heated to 150°C, and continued to be heated at a vacuum degree of 0.09 MPa to remove the solvent and small molecule impurities; when the solvent and small molecules are basically removed, a light yellow transparent titanium-containing modified silicone resin prepolymer is obtained.
[0092] (3) Preparation of UV-curable modified silicone resin
[0093] Take 50 parts of the titanium-containing modified silicone resin prepolymer prepared in the above step (2), add 1.5 parts of xanthenylphenyl iodonium salt as a photoinitiator; use a stirrer to fully stir the mixture to ensure that the photoinitiator is evenly dispersed in the resin; then degas the stirred mixture to remove bubbles generated during the mixing process to ensure that the surface of the cured product is smooth and defect-free; place the degassing mixture in an ultraviolet light curing device and perform light curing under ultraviolet light; finally, adjust the intensity and irradiation time of the ultraviolet light according to actual conditions until the mixture is completely cured to form a titanium-containing modified silicone resin cured product.
[0094] The properties of the modified silicone resin cured products obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were tested by the following method:
[0095] (1) Determination of sample refractive index: The refractive index of both liquid and solid samples was tested using an Abbe refractometer. The liquid sample was evenly coated on the surface of the light-transmitting sheet for testing, and the solid sample was prepared with a size of 20 mm*5 mm*0.5 mm and attached to the light-transmitting sheet for testing.
[0096] (2) Determination of curing transmittance: The test was conducted at 25°C using a UV-visible spectrophotometer with a scanning wavelength range of 300 to 800 nm.
[0097] (3) Determination of mechanical strength of cured product: The test was conducted using a Shore A hardness tester with a test sample size of 60 cm*60 cm*10 cm.
[0098] (4) Red ink contamination experiment: The LED bracket encapsulated with the packaging material is placed in a mixed solvent of red ink, alcohol and distilled water for reflux cooking. The mass ratio of the three liquids is 1:1:1. If the red ink still does not penetrate into the bracket after the cooking time exceeds 6 hours, it indicates that the packaging material and the bracket have good adhesion.
[0099] (5) High temperature and high humidity resistance test: In a constant temperature and humidity chamber at a temperature of 85°C and a humidity of 85RH, the LED lamp packaged with the packaging material is powered on and ignited to conduct a lighting test. The LED lamp current is controlled to be 350mmA and the voltage is controlled to be 12V until the lamp bead goes out.
[0100] The test results are as follows:
[0101] Refractive Index Light transmittance (%) Hardness(A) Red ink experiment High temperature and humidity resistance / h Example 1 1.72 98.4% 55 No pollution More than 1000 Example 2 1.75 98.5% 58 No pollution More than 1000 Example 3 1.68 98.8% 61 No pollution More than 1000 Example 4 1.70 99.0% 68 No pollution More than 1000 Comparative Example 1 1.52 97.0% 50 No pollution 600h Comparative Example 2 1.54 96.5% 70 pollute -
[0102] The test results show that the hardness of the modified silicone resin increases significantly with the increase of polyurethane (indirectly reflected by the addition of diisocyanate). The specific comparison is as follows: the addition of diisocyanate (polyurethane precursor) in Example 1 is 20 parts, and the hardness is 55A; the addition of diisocyanate in Example 2 is increased to 25 parts, and the hardness is increased to 58A; from Examples 1 and 2, it can be seen that the increase in the addition of polyurethane significantly increases the hardness of the resin, because the introduction of polyurethane enhances the crosslinking density inside the resin, thereby increasing its hardness.
[0103] In both Example 3 and Example 4, 1,1,3,3-tetramethyl-1,3-di-2-phenylethylated disiloxane was used as the phenyl source, but the contents were different (15 parts and 20 parts respectively); after testing, the modified silicone resin cured product of Example 3 had a refractive index of 1.68, a light transmittance of 98.8%, and a hardness of 61A. The modified silicone resin cured product of Example 4 had a refractive index of 1.70, a light transmittance of 99.0%, and a hardness of 68A. It can be seen that the increase in the phenyl content increases the hardness and light transmittance of the resin, and the introduction of the phenyl group helps to improve the optical properties and physical properties of the resin.
[0104] The modified silicone resin preparation methods provided in Examples 1 to 4 all added titanium, and the high temperature and high humidity resistance was more than 1000 hours. The preparation method of Comparative Example 1 did not contain titanium, and the high temperature and high humidity resistance was 600 hours; thus, it can be seen that the addition of titanium significantly improved the high temperature and high humidity resistance of the modified silicone resin.
[0105] The preparation method of comparative example 2 does not contain polyurethane, and the red ink test results show contamination, indicating that the adhesion between the packaging material and the bracket is poor; the preparation methods of embodiments 1 to 4 all contain polyurethane, and they all show "no contamination" in the red ink test, indicating that the packaging material and the bracket have good adhesion. It can be seen that polyurethane can improve the adhesion between the packaging material and the bracket.
[0106] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all these improvements and changes should fall within the scope of protection of the appended claims of the present invention.
[0107] The above is an exemplary description of the present invention. Obviously, the implementation of the present invention is not limited to the above method. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for preparing a modified silicone resin for LED packaging, characterized in that: The following steps are involved: (1) Preparation of modified silicone resin prepolymer: hydrolyze polyethyl silicate, then add alcohol, ketone or ester solvent, deionized water, epoxysiloxane and diisocyanate to the hydrolyzate, then add the pre-mixed polyether diol, phenylsiloxane and end-capping agent mixture to the above reaction system in a dropwise manner to obtain a modified silicone resin prepolymer; (2) Preparation of titanium-modified silicone resin prepolymer: under nitrogen protection, titanate is slowly added dropwise to the modified silicone resin prepolymer to generate a light yellow transparent liquid; the light yellow transparent liquid is subjected to a reduced pressure and temperature treatment to remove the solvent and small molecular impurities to obtain a titanium-containing modified silicone resin prepolymer; (3) UV curing: The titanium-containing modified silicone resin prepolymer and the photoinitiator are mixed in proportion and stirred evenly, and then the evenly stirred mixture is degassed. The degassed mixture can be photocured under ultraviolet light to form a titanium-containing modified silicone resin cured product.
2. The method for preparing a modified silicone resin for LED packaging according to claim 1, characterized in that: In step (1), the preparation process of the modified silicone resin prepolymer is specifically as follows: a. Hydrolyze polyethyl silicate under acidic or alkaline conditions at 0-10°C for 0.5-1h; b. Add alcohol, ketone or ester solvent, deionized water, epoxysiloxane and diisocyanate to the hydrolyzate obtained in step a, maintain the temperature of the reaction system between 10° C. and 20° C., and continue stirring the reaction for 0.5 h to 1 h; c. Add the pre-mixed polyether diol, phenylsiloxane and end-capping agent mixture dropwise to the reaction system obtained in step b within 10 to 30 minutes, then heat the reaction system to 70 to 100° C. and keep the reaction within this temperature range for 3 to 6 hours to complete the grafting and polymerization reaction; d. After the reaction is completed, the reaction mixture is cooled to room temperature and subjected to extraction and separation using an aromatic solvent. The lower layer of liquid after the extraction and separation is taken and subjected to neutralization and water removal treatment to obtain a modified silicone resin prepolymer.
3. The method for preparing a modified silicone resin for LED packaging according to claim 2, characterized in that: In step (2), the preparation process of the titanium-modified silicone resin prepolymer is specifically as follows: e. Under nitrogen protection, the modified silicone resin prepolymer prepared in step d is placed in a reaction container, and titanate is slowly added thereto; the temperature of the reaction system is controlled at 60° C., and the temperature is maintained for 6 hours, during which nitrogen is continuously introduced to maintain an inert atmosphere, and the reaction generates a light yellow transparent liquid; f. The light yellow transparent liquid obtained in step e is subjected to a reduced pressure and temperature treatment, and desolventizing and small molecule reaction are carried out at 150° C. and a pressure of 0.09 MPa to remove unreacted titanate, solvent and other small molecule impurities to obtain a modified silicone resin prepolymer containing titanium.
4. The method for preparing a modified silicone resin for LED packaging according to claim 2, characterized in that: The ingredients of the modified silicone resin prepolymer are added in the following proportions: 2-3 parts of acidic or alkaline catalyst; 100-150 parts of polyethyl silicate; 10-20 parts of alcohol / ketone / ester solvent; 10-20 parts of deionized water; 10-20 parts of epoxysiloxane; 20-40 parts of diisocyanate; 20-40 parts of polyether diol; 10-30 parts of phenylsiloxane; 20-40 parts of end-capping agent; 40-50 parts of xylene.
5. The method for preparing a modified silicone resin for LED packaging according to claim 2, characterized in that: The polyether diol is selected from one or more of PEG200, PEG400, PEG600, PEG800, PEG1000, PEG5000 and PEG10000.
6. The method for preparing a modified silicone resin for LED packaging according to claim 2, characterized in that: The diisocyanate is preferably one or more of toluene diisocyanate, diphenylmethane diisocyanate, naphthalene diisocyanate and hexamethylene diisocyanate.
7. The method for preparing a modified silicone resin for LED packaging according to claim 2, characterized in that: The catalyst includes an acidic catalyst or a basic catalyst. The acidic catalyst includes hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, phosphorous acid, hypophosphorous acid, iodic acid or superphosphoric acid; the basic catalyst includes sodium hydroxide, potassium hydroxide, aluminum hydroxide, sodium bicarbonate, ammonium bicarbonate, sodium carbonate or tetramethylammonium hydroxide.
8. The method for preparing a modified silicone resin for LED packaging according to claim 2, characterized in that: The capping agent has a structure of (CH3)2R1SiOSiR2(CH3)2, wherein R1 and R2 are CH3 and phenyl, respectively.
9. The method for preparing a modified silicone resin for LED packaging according to claim 3, characterized in that: The titanate is one or more of tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, n-butyl titanate, tetraisobutyl titanate, di(acetylacetonato)diisopropyl titanate, isopropoxy tri(dioctyl phosphate) titanate, isopropyl trioleyl titanate, and isopropyl triisostearate titanate; the addition amount of the titanate is 0.5-1% of the total amount of the modified silicone resin prepolymer.
10. The method for preparing a modified silicone resin for LED packaging according to claim 3, characterized in that: The photoinitiator is one or more of xanthenyl phenyl iodonium salt, fluorenyl phenyl iodonium salt, isopropylbenzene (II) hexafluorophosphate, dialkylbenzoyl sulfonium salt, triaryl (1-pyrene) bismuthium salt, dialkylbenzoyl sulfonium salt, dialkylbenzoyl sulfonium salt, bis(5-fluorothiophene-2-yl) iodonium formate, S,S-dialkyl-S-(dimethylhydroxyphenyl) sulfonium salt and phenylthiophenyl diphenyl sulfonium salt; the added amount of the photoinitiator is 1-3% of the total amount of the titanium-containing modified silicone resin prepolymer.