Preparation method of functionalized UiO-66 for ammonia gas adsorption
By using raw materials such as zirconium chloride, 2,5-dihydroxyterephthalic acid and acetic acid in the preparation of UiO-66 materials, combined with benzyl alcohol and formic acid, the coordination environment is regulated, and the porosity of functionalized UiO-66 has been successfully improved. and adsorption performance solves the shortcomings of existing materials in ammonia adsorption separation, and achieves high-efficiency ammonia adsorption and excellent adsorption selectivity.
Patent Information
- Application Number
- CN202411205444.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing functionalized UiO-66 materials have problems with insufficient porosity and specific surface area during the ammonia adsorption and separation process, resulting in poor adsorption performance and selectivity.
Zirconium chloride and 2,5-dihydroxyterephthalic acid are used as raw materials, combined with acetic acid and DMF solvents, and different contents of benzyl alcohol and formic acid are added. Through ultrasonic treatment and solvent thermal reaction, the crystallization rate and coordination environment are regulated. The unstable ligand was then removed with hydrochloric acid to prepare a high yield and high crystallinity UiO-66-(OH)2 material.
It improves the porosity, specific surface area and synthesis stability of the material, maintains the ultra-microporous structure, and significantly improves the ammonia adsorption performance and selectivity.
Smart Images

Figure CN118930892A_ABST
Abstract
Description
Technical Field
[0001] The present invention specifically relates to a method for preparing functionalized UiO-66 for ammonia adsorption, and belongs to the field of toxic and harmful gas adsorption and purification. Background Art
[0002] Ammonia is a typical alkaline gas that is polluting and highly corrosive, which is extremely harmful to the human body and the environment. At the same time, as a carbon-free hydrogen energy carrier, the development of efficient ammonia storage technology to carry hydrogen is an effective means to reduce carbon dioxide emissions, which is of great significance to achieving the "dual carbon" goal. In recent years, metal-organic framework materials (MOFs) have attracted widespread attention as a highly potential adsorption and purification material for toxic and harmful gases. Among them, zirconium-based MOFs are widely used in the separation of various small molecule gases due to the stability of their Zr-O bonds, especially in the adsorption of ammonia, which can effectively reduce the attack of ammonia with lone pairs of electrons on the coordination bonds between metals and ligands, and maintain the stability of the structure.
[0003] In the synthesis of MOFs, the selection of organic ligands with functional groups can synthesize MOFs with unique functions in situ. Functionalized MOFs materials can be applied to different aspects by utilizing the properties of different functional groups, but there are problems such as poor crystallinity and unstable products in the preparation process. In addition, the study of the article with DOI 10.1016 / j.ces.2014.08.050 shows that when UiO-66 is functionalized by introducing large functional groups, the large surface groups will block the small gaps in the skeleton, resulting in a decrease in the porosity and specific surface area of the material. In response to these problems, many researchers have used defect engineering to improve the porosity and adsorption sites of the materials. For example, the article with DOI 10.1039 / D2EN01035F prepared a series of hierarchical porous MOFs materials through competitive coordination, but the mesoporous and macroporous structures will lead to reduced selectivity in some gas adsorption and separation processes. Therefore, while improving the specific surface area and porosity of functionalized zirconium-based MOFs, improving the crystallinity of the material, preparation stability and maintaining suitable pore cages are the key to improving gas adsorption and separation. Summary of the invention
[0004] The purpose of the present invention is to improve the porosity, specific surface area and synthetic stability of functionalized UiO-66 while maintaining the ultra-microporous structure to solve the above-mentioned problems, thereby improving the application of functionalized UiO-66 in ammonia adsorption and separation.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a UiO-66-(OH)2 metal organic framework material with high yield, high crystallinity, large specific surface area and ultra-microporous structure. The material is made of zirconium chloride and 2,5-dihydroxyterephthalic acid as raw materials, acetic acid and DMF as solvents, different amounts of benzyl alcohol and formic acid are added, the two act synergistically to regulate the crystallization rate and coordination environment, and then the target product is obtained by removing unstable ligands with hydrochloric acid.
[0007] The specific preparation method comprises the following steps:
[0008] Step 1, dispersing zirconium chloride, 2,5-dihydroxyterephthalic acid and acetic acid in DMF, and magnetically stirring for 30 minutes until the solid is completely dissolved;
[0009] Step 2, adding a small amount of benzyl alcohol and formic acid to the above solution, ultrasonically treating for 10 to 30 minutes to evenly disperse the solvent, and then subjecting the mixed solution to a solvothermal reaction at 100 to 150° C.;
[0010] Step 3, after the reaction is cooled to room temperature, the supernatant is discarded, and the obtained solid material is soaked in a mixed solution of hydrochloric acid and DMF for 1 to 6 hours, washed with DMF and methanol for 3 to 6 times respectively, centrifuged and vacuum dried to obtain UiO-66-(OH)2;
[0011] Preferably, in step 1, the molar ratio of zirconium chloride, 2,5-dihydroxyterephthalic acid and acetic acid is 1:1:40; the molar ratio of zirconium chloride and DMF is 1:250;
[0012] Preferably, in step 2, the molar ratio of zirconium chloride to benzyl alcohol is 1:20; the molar ratio of zirconium chloride to formic acid is 1:10;
[0013] Preferably, the ultrasonic treatment time in step 2 is 20 min;
[0014] Preferably, the solvent thermal reaction temperature in step 2 is 120° C. and the insulation time is 24 h;
[0015] Preferably, the volume of the mixed solution in step 3 is 50 mL; the volume percentage of hydrochloric acid is 10%; and the soaking time is 2 h;
[0016] Preferably, in step 3, the DMF and methanol are washed three times respectively; and vacuum dried at 60° C. for 12 h;
[0017] Finally, the UiO-66-(OH)2 metal organic framework material can be obtained with a yield of more than 78wt%.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention prepares functionalized UiO-66 with high crystallinity and stable product through the synergistic effect of lower alcohol and monocarboxylic acid ligand, which is conducive to large-scale production and preparation;
[0020] (2) The present invention can improve the problem of small voids in the skeleton being blocked due to the introduction of large functional groups, thereby increasing the specific surface area and porosity of the material while maintaining the ultra-microporous structure;
[0021] (3) The preparation method of the present invention is simple, energy-saving and environmentally friendly, can effectively improve the ammonia adsorption performance and has excellent adsorption selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The X-ray powder diffraction (XRD) patterns of the samples obtained in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 are shown.
[0023] Figure 2 Polarized light microscope images of the samples obtained in Example 1, Example 2 and Example 3.
[0024] Figure 3 Thermogravimetric analysis (TGA) curves of the samples obtained in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 are shown.
[0025] Figure 4 The adsorption-desorption curves and pore size distribution diagrams of the samples obtained in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 are shown.
[0026] Figure 5 It is a performance evaluation diagram of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 in ammonia adsorption.
[0027] Figure 6 This is a graph evaluating the adsorption selectivity of carbon dioxide and nitrogen for the sample obtained in Example 1. DETAILED DESCRIPTION
[0028] The present invention is further described below in conjunction with the accompanying drawings, embodiments and comparative examples. The specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0029] Example 1
[0030] Step 1, 668 mg of zirconium chloride, 500 mg of 2,5-dihydroxyterephthalic acid and 6.6 mL of acetic acid were dispersed in 50 mL of DMF and magnetically stirred for 30 min until the solid was completely dissolved;
[0031] Step 2, then add 3 mL of benzyl alcohol and 1 mL of formic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0032] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of hydrochloric acid and DMF for 2 hours, the volume of the mixed solution is 50mL, and the volume percentage of hydrochloric acid is 10%. After centrifugation, DMF and methanol washing for 3 times respectively, vacuum drying at 60°C for 12 hours, the target product UiO-66-(OH)2 is obtained.
[0033] Example 2
[0034] Step 1, 668 mg of zirconium chloride, 500 mg of 2,5-dihydroxyterephthalic acid and 6.6 mL of acetic acid were dispersed in 50 mL of DMF and magnetically stirred for 30 min until the solid was completely dissolved;
[0035] Step 2, then add 3 mL of benzyl alcohol and 0.5 mL of formic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0036] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of hydrochloric acid and DMF for 2 hours, the volume of the mixed solution is 50mL, and the volume percentage of hydrochloric acid is 10%. After centrifugation, DMF and methanol washing for 3 times respectively, vacuum drying at 60°C for 12 hours, the target product UiO-66-(OH)2 is obtained.
[0037] Example 3
[0038] Step 1, 668 mg of zirconium chloride, 500 mg of 2,5-dihydroxyterephthalic acid and 6.6 mL of acetic acid were dispersed in 50 mL of DMF and magnetically stirred for 30 min until the solid was completely dissolved;
[0039] Step 2, then add 3 mL of benzyl alcohol and 2 mL of formic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0040] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of hydrochloric acid and DMF for 2 hours, the volume of the mixed solution is 50mL, and the volume percentage of hydrochloric acid is 10%. After centrifugation, DMF and methanol washing for 3 times respectively, vacuum drying at 60°C for 12 hours, the target product UiO-66-(OH)2 is obtained.
[0041] Example 4
[0042] Step 1, 600 mg of zirconium oxychloride, 458.4 mg of 2-sulfonate terephthalic acid and 4.3 mL of acetic acid were dispersed in 60 mL of DMF and magnetically stirred for 30 min until the solid was completely dissolved;
[0043] Step 2, then add 2 mL of anhydrous ethanol and 1.8 mL of benzoic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 130° C. for 24 hours.
[0044] Step 3, after the reaction is completed, the mixture is cooled to room temperature naturally, the supernatant is discarded, and the obtained solid material is soaked in a mixed solution of nitric acid and DMF for 3 hours, the volume of the mixed solution is 50 mL, and the volume percentage of nitric acid is 10%. After centrifugation, DMF and methanol washing are performed 4 times respectively, and vacuum drying is performed at 60°C for 12 hours to obtain the target product UiO-66-SO3H.
[0045] Example 5
[0046] Step 1, 600 mg of zirconium nitrate, 435.4 mg of 2-sulfonatoterephthalic acid and 4 mL of acetic acid were dispersed in 60 mL of DMF and magnetically stirred for 30 min until the solid was completely dissolved;
[0047] Step 2, then add 2.1 mL of methanol and 4 mL of lactic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 150° C. for 12 hours.
[0048] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of hydrochloric acid and DMF for 6 hours, the volume of the mixed solution is 60 mL, and the volume percentage of hydrochloric acid is 5%. After centrifugation, DMF and methanol washing for 3 times respectively, vacuum drying at 80°C for 12 hours, the target product UiO-66-SO3H is obtained.
[0049] Example 6
[0050] Step 1, 500 mg of zirconium oxychloride, 282.6 mg of 2-hydroxyterephthalic acid and 3.5 mL of acetic acid were dispersed in 50 mL of DMF and magnetically stirred for 30 min until the solid was completely dissolved;
[0051] Step 2, then add 2.3 mL of propanol and 3.5 mL of citric acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0052] Step 3, after the reaction is completed, the mixture is cooled to room temperature naturally, the supernatant is discarded, and the obtained solid material is soaked in a mixed solution of sulfuric acid and DMF for 4 hours, the volume of the mixed solution is 60 mL, and the volume percentage of sulfuric acid is 5%. After centrifugation, DMF and methanol washing for 3 times respectively, and vacuum drying at 60°C for 12 hours, the target product UiO-66-OH is obtained.
[0053] Example 7
[0054] Step 1, disperse 500 mg of zirconium chloride, 390.8 mg of 2-hydroxyterephthalic acid and 5 mL of acetic acid in 50 mL of DMF, and stir magnetically for 30 min until the solid is completely dissolved;
[0055] Step 2, then add 1.2 mL of ethylene glycol and 1.6 mL of trifluoroacetic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0056] Step 3, after the reaction is completed, the mixture is cooled to room temperature naturally, the supernatant is discarded, and the obtained solid material is soaked in a mixed solution of sulfuric acid and DMF for 4 hours, the volume of the mixed solution is 60 mL, and the volume percentage of sulfuric acid is 10%. After centrifugation, DMF and methanol washing for 3 times respectively, and vacuum drying at 60°C for 12 hours, the target product UiO-66-OH is obtained.
[0057] Example 8
[0058] Step 1, disperse 500 mg of zirconium chloride, 545.3 mg of 1,2,4,5-benzenetetracarboxylic acid and 5 mL of acetic acid in 50 mL of DMF, and stir magnetically for 30 min until the solid is completely dissolved;
[0059] Step 2, then add 3.2 mL of propylene glycol and 6.5 mL of salicylic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0060] Step 3, after the reaction is completed, the mixture is cooled to room temperature naturally, the supernatant is discarded, and the obtained solid material is soaked in a mixed solution of oxalic acid and DMF for 4 hours, the volume of the mixed solution is 60 mL, and the volume percentage of oxalic acid is 15%. After centrifugation, DMF and methanol washing are performed 4 times respectively, and vacuum drying is performed at 60°C for 12 hours to obtain the target product UiO-66-COOH.
[0061] Example 9
[0062] Step 1, disperse 650 mg of zirconium oxychloride, 365.4 mg of 2-aminoterephthalic acid and 5.8 mL of acetic acid in 60 mL of DMF and stir magnetically for 30 min until the solid is completely dissolved;
[0063] Step 2, then add 2.4 mL of anhydrous ethanol and 3 mL of succinic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution to a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 120° C. for 24 hours.
[0064] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of nitric acid and DMF for 4 hours, the volume of the mixed solution is 60mL, and the volume percentage of nitric acid is 20%. After centrifugation, DMF and methanol washing 6 times respectively, vacuum drying at 80°C for 6 hours to obtain the target product UiO-66-NH2.
[0065] Example 10
[0066] Step 1, disperse 560 mg of zirconium nitrate, 348.5 mg of 2-nitroterephthalic acid and 3.8 mL of acetic acid in 50 mL of DMF and stir magnetically for 30 min until the solid is completely dissolved;
[0067] Step 2, then add 2 mL of methanol and 1.6 mL of benzoic acid, ultrasonicate for 20 min to obtain a mixed solution, transfer the obtained mixed solution into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave, and keep it at 150° C. for 24 hours.
[0068] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of hydrochloric acid and DMF for 1 hour, the volume of the mixed solution is 60mL, and the volume percentage of hydrochloric acid is 15%. After centrifugation, DMF and methanol washing for 3 times respectively, vacuum drying at 60°C for 12 hours, the target product UiO-66-NO2 is obtained.
[0069] Comparative Example 1
[0070] Step 1, 668 mg of zirconium chloride, 500 mg of 2,5-dihydroxyterephthalic acid and 6.6 mL of acetic acid are dispersed in 50 mL of DMF, and magnetically stirred for 30 min until the solid is completely dissolved to obtain a mixed solution.
[0071] Step 2: The mixed solution was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and kept at 120° C. for 24 hours.
[0072] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, wash the obtained solid material with DMF and methanol three times respectively, centrifuge and vacuum dry at 60°C for 12 hours to obtain the target product UiO-66-(OH)2.
[0073] Comparative Example 2
[0074] Step 1, 668 mg of zirconium chloride, 500 mg of 2,5-dihydroxyterephthalic acid and 6.6 mL of acetic acid are dispersed in 50 mL of DMF, and magnetically stirred for 30 min until the solid is completely dissolved to obtain a mixed solution.
[0075] Step 2: The mixed solution was transferred into a 100 mL polytetrafluoroethylene-lined stainless steel autoclave and kept at 120° C. for 24 hours.
[0076] Step 3, after the reaction is completed, cool naturally to room temperature, pour off the supernatant, soak the obtained solid material in a mixed solution of hydrochloric acid and DMF for 2 hours, the volume of the mixed solution is 50mL, and the volume percentage of hydrochloric acid is 10%. After centrifugation, DMF and methanol washing for 3 times respectively, vacuum drying at 60°C for 12 hours, the target product UiO-66-(OH)2 is obtained.
[0077] Figure 1 The X-ray powder diffraction (XRD) diagrams of the samples obtained in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 are shown in FIG. Figure 1 It can be seen that the characteristic diffraction peaks of all samples are consistent with those of the standard sample UiO-66, indicating that hydroxylated UiO-66 was successfully prepared and the material has good crystallinity. With the introduction of benzyl alcohol and formic acid, the peak width of the material characteristic peak gradually narrowed and the peak intensity increased, indicating that the crystallinity of the material was further improved.
[0078] Figure 2 The polarizing microscope images of the samples obtained in Example 1, Example 2 and Example 3 are all 10 um in scale. Figure 2 It can be seen that the UiO-66-(OH)2 sample prepared under the synergistic effect of benzyl alcohol and formic acid has good crystallinity, uniform size and high dispersion, which is consistent with the XRD results.
[0079] Figure 3 The thermogravimetric analysis curves (TGA) of the samples obtained in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 are shown in FIG. Figure 3 It can be seen that all samples have similar two-stage weightlessness platform temperatures, indicating that the samples have the same thermal stability. Comparative Examples 1 and 2 have fewer defects because no additional monocarboxylic acid ligands are added. However, Examples 1, 2, and 3, which add benzyl alcohol and different proportions of formic acid, have more ligand defect sites, which plays an important role in improving the adsorption performance of ammonia.
[0080] Figure 4 The adsorption-desorption curves and pore size distribution diagrams of the samples obtained in Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 show that the N2 adsorption-desorption curves of all samples show obvious type I isotherm characteristics, indicating that the pore structure of the material is mainly a microporous structure, which is consistent with the pore size distribution curve results.
[0081] The results are analyzed as shown in Table 1. Compared with the comparative example, the synergistic effect of benzyl alcohol and formic acid can effectively stabilize the precursor, make the material more crystallinity, and have a uniform pore size distribution. After the unstable ligands are removed by acid, more defect sites are generated, which increases the specific surface area and pore volume of the material, up to 1180.5 m 2 / g and 0.57cm 3 / g. In addition, the specific surface area and pore volume are increased while maintaining the ultra-microporous structure, which plays an important role in improving the ammonia adsorption selectivity.
[0082]
[0083] Table 1
[0084] Figure 5 The ammonia adsorption test results of Example 1, Example 2, Example 3, Comparative Example 1 and Comparative Example 2 at room temperature and pressure, with a concentration of 1000000 ppm and a flow rate of 20 mL / min, can be seen that Example 1 with a larger specific surface area and pore volume has the best ammonia adsorption effect, and the saturated adsorption amount is 200 mg / g.
[0085] Figure 6 This is an evaluation diagram of the adsorption selectivity of carbon dioxide and nitrogen obtained by the sample obtained in Example 1. Under the same reaction conditions, Example 1 with an ultra-microporous structure hardly adsorbs CO2 and N2, indicating that it has excellent adsorption selectivity for ammonia.
[0086] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing functionalized UiO-66 for ammonia adsorption, characterized in that: The preparation method comprises the following steps: Step 1, dispersing the zirconium source, functionalized terephthalic acid and acetic acid in DMF, stirring evenly until the solid is completely dissolved to obtain a mixed solution; Step 2, adding the lower alcohol and the monocarboxylic acid ligand to the mixed solution, further mixing by ultrasonic treatment, and then performing a solvothermal reaction; Step 3: After the solvothermal reaction is completed, the layers are allowed to stand and the supernatant is discarded. The obtained solid material is soaked in a solution including an acid and DMF, and then washed with DMF and methanol respectively, and then centrifuged and vacuum dried to obtain the functionalized UiO-66.
2. The preparation method according to claim 1, characterized in that: The zirconium source includes one or more of zirconium chloride, zirconium oxychloride and zirconium nitrate; The functionalized terephthalic acid includes one of 2,5-dihydroxyterephthalic acid, 2-hydroxyterephthalic acid, 2-sulfonic terephthalic acid, 1,2,4,5-benzenetetracarboxylic acid, 2-nitroterephthalic acid and 2-aminoterephthalic acid; The lower alcohol includes one or more of benzyl alcohol, methanol, ethanol, propanol, ethylene glycol and propylene glycol; The monocarboxylic acid ligand includes one or more of formic acid, benzoic acid, citric acid, succinic acid, salicylic acid, lactic acid and trifluoroacetic acid; The acid includes one or more of hydrochloric acid, sulfuric acid, nitric acid and oxalic acid.
3. The preparation method according to claim 1, characterized in that: The molar ratio of the zirconium source, functionalized terephthalic acid and acetic acid is (1-1.5): (1-1.5): (30-50); The molar ratio of the zirconium source to DMF is 1:(240-280), the molar ratio of the zirconium source to the lower alcohol is 1:(10-30), and the molar ratio of the zirconium source to the monocarboxylic acid ligand is 1:(5-30); The volume of the solution including the acid and DMF is 40-100 mL, wherein the volume percentage of the acid is 5-20%.
4. The preparation method according to claim 1, characterized in that: In the step 2, the ultrasonic treatment time is 10-30 min.
5. The preparation method according to claim 1, characterized in that: In the step 2, the temperature of the solvent thermal reaction is 100-150° C., and the insulation time is 12-36 hours.
6. The preparation method according to claim 1, characterized in that: In the step 3, the solid material is soaked in the solution including acid and DMF for 1-6 hours.
7. The preparation method according to claim 1, characterized in that: In the step 3, the DMF and methanol washing times are 3-6 times.
8. The preparation method according to claim 1, characterized in that: In step 3, the vacuum drying temperature is 50-80° C., and the drying time is 8-24 hours.
9. Functionalized UiO-66 prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the functionalized UiO-66 according to claim 9 for adsorption and separation of ammonia with a concentration of 1000ppm-1000000ppm at normal temperature and pressure.
Citation Information
Patent Citations
Preparation method for synthesizing metal organic framework UiO-66 adsorbents by aid of mixed ligands
CN109395698A
Method for preparing UiO-66 based on benzoic acid regulation and chloroform activation and adsorption application
CN109589934A
Ce-based organic metal complex catalytic material and preparation method and application thereof
CN111450894A
Super-microporous hydrophobic UiO-66 zirconium metal organic framework material as well as preparation method and application thereof
CN112979978A
General preparation method of multistage porous metal organic framework material
CN113773517A
Cited By
Hydrogen bond molecular crystal material for ammonia trapping as well as preparation method and application of hydrogen bond molecular crystal material
CN121699173A