Preparation method of hydrophilic monodisperse carboxyl magnetic microspheres
By adding crosslinking agent, sulfonation treatment, coating silica and surface modified carboxylic groups in the preparation process of magnetic microspheres, the problem of dissolution or fragmentation of existing magnetic microspheres in non-polar solutions is solved, and the problem of improvement of existing magnetic microspheres is improved Magnetic response speed and dispersion uniformity achieve more stable magnetic properties.
Patent Information
- Application Number
- CN202411184280.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
AI Technical Summary
Existing magnetic microspheres are easily dissolved or fragmented in non-polar solutions, and magnetic particles are easily shedded and agglomerated in co-precipitation magnetization methods, and the magnetic response speed is insufficient, making it difficult to disperse evenly.
Solid polystyrene microspheres were prepared by dispersing polymerization, and crosslinking agent was added during the polymerization process, and iron ions were adsorbed, silica was coated, and carboxyl groups were modified on the surface to improve the crosslinking degree of microspheres and Magnetic responsiveness.
The microspheres maintain rigidity and integrity in non-polar solutions are solved, which enhances the stability and dispersion uniformity of magnetic particles, and improves the magnetic response speed and hydrophilic properties.
Smart Images

Figure CN118930906A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of magnetic materials, and in particular to a method for preparing hydrophilic monodisperse carboxyl magnetic microspheres. Background Art
[0002] Magnetic polymer microspheres, referred to as magnetic microspheres, are a new type of magnetic material developed in recent years. They are composite microspheres with certain magnetism and special structures formed by combining magnetic inorganic particles with organic polymers by appropriate methods. Magnetic composite microspheres not only have many characteristics of ordinary polymer microspheres but also have magnetic responsiveness. Therefore, they can not only be endowed with surface functional groups (such as -OH, -COOH, -CHO, -NH2, etc.) through copolymerization and surface modification, but also have a guiding function under the action of an external magnetic field.
[0003] At present, the common methods for synthesizing magnetic microsphere templates mainly include emulsion polymerization, suspension polymerization, seed swelling polymerization and dispersion polymerization. Among them, dispersion polymerization and seed swelling polymerization are more widely used, especially dispersion polymerization. Dispersion polymerization can synthesize polymer microspheres with a particle size of 1 to 20 μm and good monodispersity. Compared with other methods, the particle size distribution of polymers synthesized by dispersion polymerization is more uniform and more controllable. Moreover, dispersion polymerization can be used for the polymerization of multiple monomers, and more types of monomers are applicable.
[0004] However, conventional dispersion polymerization and seed swelling polymerization still show some shortcomings in practical applications: when synthesizing microsphere templates, dispersion polymerization adds polymer monomers, stabilizers and a certain amount of initiators to the solvent system, and reacts at a certain temperature to obtain microspheres with uniform particle size, but the microspheres are not cross-linked and are easily dissolved in non-polar solutions; seed swelling polymerization is based on the seeds of dispersion polymerization, first swelling the seeds with an activator, and then adding monomers, pore-forming agents, cross-linking agents, etc., to allow the small seeds to swell into larger uniform microspheres. Although the microspheres are cross-linked and can maintain rigidity in non-polar solutions, they have a porous structure and high rigidity, and are easily broken in non-polar solvents and during ultrasound.
[0005] In addition, regarding the magnetization methods of monodisperse magnetic microspheres, there are currently hydrothermal method, solvothermal method, coprecipitation method, etc. Among them, the magnetized microspheres prepared by hydrothermal method and solvothermal method are uniform and have high magnetic content, but the disadvantage is that the reaction environment is high temperature and high pressure, and the yield is extremely low; the coprecipitation method is simple, it is easy to form a coating on the surface of the microspheres, the reaction environment can be at room temperature, and it is easy to produce and scale up, but the disadvantage is that the microspheres are easy to fall off and agglomerate during the dispersion process, the magnetic response speed is insufficient, or it is difficult to disperse evenly. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a new preparation method for hydrophilic monodisperse carboxyl magnetic microspheres, so as to avoid the problems that the microspheres are easily dissolved in non-polar solutions or broken in non-polar solvents and during ultrasound when preparing microsphere templates by the existing dispersion polymerization method and seed swelling polymerization method, and the problems that the magnetic particles are easy to fall off and agglomerate, the magnetic response speed is insufficient, and it is difficult to disperse uniformly when magnetizing the microspheres by the existing co-precipitation magnetization method.
[0007] The present invention adopts the following technical solutions to solve the above technical problems:
[0008] A method for preparing hydrophilic monodisperse carboxyl magnetic microspheres comprises the following steps:
[0009] (1) Microsphere template synthesis
[0010] Monodisperse microsphere templates were prepared by dispersion polymerization, and solid polystyrene microspheres were obtained by adding a cross-linking agent during the polymerization process.
[0011] (2) Microsphere magnetization
[0012] The surface of the microspheres is sulfonated to make the microspheres negatively charged; then the negatively charged microspheres are used to adsorb positively charged iron ions and ferrous ions to complete the magnetization of the microspheres;
[0013] (3) Surface coating of magnetic microspheres
[0014] The surface of the magnetic microspheres is coated with silicon dioxide, and then solidified to obtain magnetic microspheres coated with silicon dioxide;
[0015] (4) Surface functionalization of magnetic microspheres
[0016] After the surface of the magnetic microspheres wrapped with silica is coated with polymer, the surface is then modified with carboxyl groups.
[0017] As one of the preferred embodiments of the present invention, in step (1), the specific process of synthesizing the microsphere template is as follows:
[0018] ①Put deionized water, anhydrous ethanol and stabilizer into a three-necked flask and place it in a water bath;
[0019] ②Introduce nitrogen into the three-necked flask and control the temperature inside the three-necked flask to 68-70°C;
[0020] ③Take styrene, add azobisisobutyronitrile, stir evenly; pour the mixture into a three-necked flask and react;
[0021] ④ Take the cross-linking agent, add ethanol and thiol compound to mix; after styrene reacts for 2 to 4 hours, drip the cross-linking agent, ethanol and thiol compound mixture (to prevent microspheres from agglomerating during the polymerization process) into the three-necked flask through a peristaltic pump;
[0022] ⑤Continue the reaction until the entire reaction is completed;
[0023] ⑥ Pour the reactants into a centrifuge bottle, centrifuge and discard the supernatant; add ethanol to ultrasonically clean the precipitated microspheres until they are dispersed, centrifuge, and repeat once; add ethanol, mix the microspheres and add them to a single-necked flask; rotary evaporate the microspheres until dry, and put them in an oven to dry overnight to obtain the solid polystyrene microspheres required for the target.
[0024] As one of the preferred embodiments of the present invention, the stabilizer is pvp K88.
[0025] As one of the preferred embodiments of the present invention, the crosslinking agent is selected from one or more of divinylbenzene (DVB) and ethylene glycol dimethacrylate (EGDMA).
[0026] As one of the preferred embodiments of the present invention, the obtained polystyrene microspheres have a particle size of 1 um.
[0027] As one of the preferred embodiments of the present invention, in step (2), the specific process of magnetizing the microspheres is as follows:
[0028] ① Weigh the dried polystyrene microspheres, put them into a beaker, add acetic acid or ethylene dichloride, and crush them in an ultrasonic crusher;
[0029] ②After the ultrasound is completed, pour the solution into a three-necked flask, rinse the beaker with acetic acid, and add it to the three-necked flask;
[0030] ③ Place the three-necked flask in an oil bath at 70-100℃ and heat it, then add concentrated sulfuric acid or acetic acid to react, wash with clean water until the supernatant does not turn red when tested with pH paper; test the sulfonate ion density to be 1.4-3.6mmol / g; put the microspheres in an oven to dry;
[0031] ④ Repeat the above step ③ several times with the dried microspheres to detect the density of the microspheres after multiple sulfonation;
[0032] ⑤ Take the sulfonated microspheres, add ferrous chloride tetrahydrate, ferric chloride pentahydrate and water, mix, and stir with ultrasound;
[0033] ⑥ Heat the solution to 75-85°C to remove the hydrochloric acid in the solution, cool it to room temperature and continue stirring;
[0034] ⑦ Add ammonia water and heat to 75-85℃ for reaction.
[0035] As one of the preferred embodiments of the present invention, in step (2) ⑤, 10 g of sulfonated microspheres, 2.69 g of ferrous chloride tetrahydrate, 7.31 g of ferric chloride pentahydrate, and 100 mL of water are used.
[0036] As one of the preferred embodiments of the present invention, in step (3), the specific process of coating the surface of the magnetic microspheres is as follows:
[0037] ① Prepare an ethanol solution containing PVP K88, add PVA aqueous solution to prepare an 80% ethanol aqueous solution; pour the magnetized microspheres into the 80% ethanol aqueous solution to obtain a magnetic microsphere solution;
[0038] ② Add ammonia water, sonicate until the microspheres are monodispersed, add silane coupling agent, and react overnight at room temperature;
[0039] ③ Centrifuge the magnetic microspheres, wash with ethanol solution until the supernatant is transparent, and dry them in a drying oven to obtain magnetic microspheres coated with silica.
[0040] As one of the preferred embodiments of the present invention, the silane coupling agent is selected from one or more of tetraethyl orthosilicate, KH550, and trimethylchlorosilane.
[0041] As one of the preferred embodiments of the present invention, in step (4), the specific process of functionalizing the surface of the magnetic microspheres is as follows:
[0042] ① Take the magnetic microspheres wrapped with silica, add dimethyl sulfoxide, and disperse them by ultrasonication; then, add ethylene dichloride to prepare a magnetic microsphere solution, add diethylene glycol glycidyl ether and glycolic acid, and stir and disperse;
[0043] ② Add boron trifluoride etherate and react;
[0044] ③ After the reaction is completed, the magnetic microspheres are taken out, washed with ethanol, and then washed with PBS buffer to obtain the desired hydrophilic monodisperse carboxyl magnetic microspheres.
[0045] The advantages of the present invention compared to the prior art are:
[0046] (1) With regard to the synthesis of microspheres, the present invention improves on the basis of dispersion polymerization, and adds a certain amount of crosslinking agent during the polymerization process to prepare solid crosslinked polystyrene microspheres, so that the microspheres are not crosslinked inside, but highly crosslinked outside, while maintaining the uniformity of the microspheres; based on this, the microspheres of the present invention can maintain rigidity in non-polar solutions and maintain a certain elastic integrity structure under many extreme conditions, thereby solving the problem that microspheres of existing dispersion polymerization and seed swelling polymerization methods are easily dissolved in non-polar solutions or broken in non-polar solvents and during ultrasound;
[0047] (2) For the magnetization of microspheres, the present invention performs multiple sulfonation on the microspheres based on the coprecipitation method, so that the microspheres can adsorb more ferric ions and ferrous ions, so that more magnetic particles are fixed on the microspheres in a more stable form and are not easy to fall off, and the magnetic response speed is enhanced, thereby solving the problems of easy falling off and agglomeration of magnetic particles and insufficient magnetic response speed in the existing coprecipitation magnetization method;
[0048] (3) For the surface coating of magnetic microspheres, the present invention adds a high viscosity stabilizer (PVPK88) during the silicon coating process, which can reduce the speed of silica gel cross-linking. At the same time, the magnetic particles are dispersed in the high viscosity stabilizer by ultrasound to form monodisperse magnetic beads, solving the problem that the existing co-precipitation magnetization method is difficult to disperse uniformly. Finally, a high temperature treatment step is performed to further cross-link the residual silicon hydroxyl groups on the surface to prevent the magnetic particles from falling off.
[0049] (4) For the functionalization of the surface of magnetic microspheres, the current mainstream coating method is mainly to coat with silica gel and then modify a layer of carboxyl groups on the surface of the silica gel; the present invention coats a layer of polymer on the basis of silica gel, modifies a layer of carboxyl groups on the surface of the polymer, and at the same time increases the hydrophilicity of the microspheres, making the functional groups on the surface of the microspheres rich and not easy to fall off, and having excellent hydrophilic properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 is an electron microscope image of the PS-DVB microsphere in Example 3;
[0051] Figure 2 is an electron microscope image of the magnetic microspheres in Example 3;
[0052] Figure 3 is an electron microscopic image of the magnetic microspheres encapsulated with silicon dioxide in Example 3;
[0053] Figure 4 is an electron microscopic image of the hydrophilic monodisperse carboxyl magnetic microspheres in Example 3;
[0054] Figure 5 is a transmission electron microscopy image of the hydrophilic monodisperse carboxyl magnetic microspheres in Example 3;
[0055] Figure 6 It is an electron micrograph of the microspheres of the present invention and comparative example 1 in Experimental Example 1 after being stored in a non-polar solvent and centrifuged (in the figure, Figure A is an electron micrograph of the uncrosslinked polystyrene microspheres of comparative example 1, and Figure B is an electron micrograph of the crosslinked microspheres of the present invention). DETAILED DESCRIPTION
[0056] The embodiments of the present invention are described in detail below. The embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments. At the same time, the reagents and experimental methods used in the following embodiments, unless otherwise specified, are conventional reagents or methods in the art and will not be repeated.
[0057] Example 1
[0058] A method for preparing hydrophilic monodisperse carboxyl magnetic microspheres of this embodiment comprises the following steps:
[0059] (1) Microsphere template synthesis
[0060] ① Take 1300g of anhydrous ethanol and 22.5g of pvp K88 (stabilizer) and put them into a 3L three-necked flask and place it in a water bath.
[0061] ②Introduce nitrogen into the three-necked flask, insert a 200℃ thermometer into the three-necked flask, and control the temperature inside the three-necked flask to about 68℃.
[0062] ③ Take 100g of styrene, add 1.5g of AIBN (azobisisobutyronitrile), and stir evenly; after the inside of the three-necked flask is stable, pour the styrene and other mixture into it and react for 2h.
[0063] ④ Take 20g of DVB (divinylbenzene), add 60g of ethanol and 0.1% of mercaptoethanol and mix; after styrene reacts for 2h, drip the crosslinking agent, ethanol and mercapto compound mixture into the three-necked flask at a speed of 10rmp / min through a peristaltic pump.
[0064] ⑤ Continue the reaction for 2.5h or until the whole reaction time is 6h, then take out the reaction mixture.
[0065] ⑥ Pour the reaction into a centrifuge bottle, centrifuge at 2000 rpm for 20 min, and discard the supernatant; add ethanol to ultrasonically clean the precipitated microspheres until they are dispersed, centrifuge at 2000 rpm for 10 min, and repeat once; add a small amount of ethanol, mix the microspheres and add them to a single-necked flask, rotary evaporate the microspheres until dry, and put them in a 70°C oven to dry overnight to obtain solid 1um PS-DVB microspheres.
[0066] (2) Microsphere magnetization
[0067] ① Weigh 10g of dried PS-DVB microspheres, put them into a beaker, add 100g of acetic acid or dichloroethane, and crush them in an ultrasonic crusher for 20min (ice bath, 300W power, on for 2s and off for 5s).
[0068] ② After the ultrasonic treatment, pour the solution into a three-necked flask, rinse the beaker with acetic acid, and add acetic acid to the three-necked flask until the total mass of the solution is 160 g (including 10 g of PS-DVB microspheres).
[0069] ③ Place the three-necked flask in a 70℃ oil bath and heat for 2h, then add 1mL of concentrated sulfuric acid and react for 1.5h. Wash with clean water until the supernatant does not turn red when tested with pH paper; test the sulfonate ion density to be 1.4-3.6mmol / g; dry the microspheres in a 100℃ oven overnight.
[0070] ④ Repeat the above step ③ twice with the dried microspheres to detect the density of the microspheres after multiple sulfonation.
[0071] ⑤ Take 10 g of sulfonated microspheres, add 2.69 g of ferrous chloride tetrahydrate, 7.31 g of ferric chloride pentahydrate, and 100 mL of water, and stir ultrasonically for 0.5 h.
[0072] ⑥ Heat the solution to 75°C to remove the hydrochloric acid in the solution, cool to room temperature and continue stirring for 2 hours.
[0073] ⑦ Add 20 mL of aqueous ammonia and heat to 75°C for 1 hour.
[0074] (3) Surface coating of magnetic microspheres
[0075] ① Prepare 1% PVP K88 (high viscosity stabilizer) ethanol solution, add 10% PVA aqueous solution to make 80% ethanol aqueous solution, pour the magnetized magnetic microspheres into it to make a 1% magnetic microsphere solution, and observe monodispersity under an ultrasonic microscope.
[0076] ② Add 1 times the mass of magnetic microspheres in ammonia water, sonicate until the microspheres are monodisperse, add 2 times the mass of magnetic microspheres in trimethylchlorosilane (silane coupling agent), and react at room temperature overnight.
[0077] ③ The magnetic microspheres were centrifuged, washed with 20% ethanol solution until the supernatant was transparent, and dried in a drying oven at 120° C. for 24 h to obtain magnetic microspheres coated with silica.
[0078] (4) Surface functionalization of magnetic microspheres
[0079] ① Take 1g of magnetic microspheres wrapped with silica, add 10g of dimethyl sulfoxide, and ultrasonically disperse for 10 minutes; then, add 60g of dichloroethane to make a 1% magnetic microsphere solution, add 1g of diethylene glycol glycidyl ether and 0.5g of glycolic acid, and stir to disperse.
[0080] ② After stirring at 0℃ for 30min, add 200uL of boron trifluoride ether and react at 0℃ for 24h.
[0081] ③ After the reaction is completed, the magnetic microspheres are taken out, washed twice with ethanol, and then washed twice with pH 7.0 PBS buffer to obtain the desired hydrophilic monodisperse carboxyl magnetic microspheres.
[0082] Example 2
[0083] A method for preparing hydrophilic monodisperse carboxyl magnetic microspheres of this embodiment comprises the following steps:
[0084] (1) Microsphere template synthesis
[0085] ① Put 200g of deionized water, 1500g of anhydrous ethanol and 22.5g of pvp K88 (stabilizer) into a 3L three-necked flask and place it in a water bath.
[0086] ②Introduce nitrogen into the three-necked flask, insert a 200℃ thermometer into the three-necked flask, and control the temperature inside the three-necked flask to about 70℃.
[0087] ③ Take 300g of styrene, add 1.5g of AIBN (azobisisobutyronitrile), and stir evenly; after the inside of the three-necked flask is stable, pour the styrene and other mixture into it and react for 2h.
[0088] ④ Take 60g of EGDMA (ethylene glycol dimethacrylate), add 120g of ethanol and 0.1% mercaptoethanol and mix; after styrene reacts for 4h, drip the crosslinking agent, ethanol and mercapto compound mixture into the three-necked flask at a speed of 10rmp / min through a peristaltic pump.
[0089] ⑤ Continue the reaction for 2.5h or until the whole reaction time is 6h, then take out the reaction mixture.
[0090] ⑥ Pour the reaction into a centrifuge bottle, centrifuge at 2000 rpm for 20 min, and discard the supernatant; add ethanol to ultrasonically clean the precipitated microspheres until they are dispersed, centrifuge at 2000 rpm for 10 min, and repeat once; add a small amount of ethanol, mix the microspheres and add them to a single-necked flask, rotary evaporate the microspheres until dry, and put them in a 70°C oven to dry overnight to obtain solid 1um PS-EGDMA microspheres.
[0091] (2) Microsphere magnetization
[0092] ① Weigh 10 g of dried PS-EGDMA microspheres, put them into a beaker, add 100 g of acetic acid or dichloroethane, and crush them in an ultrasonic crusher for 20 min (ice bath, 300 W power, on for 2 s and off for 5 s).
[0093] ② After the ultrasonic treatment, pour the solution into a three-necked flask, rinse the beaker with acetic acid, and add acetic acid to the three-necked flask until the total mass of the solution is 160 g (including 10 g of PS-EGDMA microspheres).
[0094] ③ Place the three-necked flask in a 100℃ oil bath and heat for 2h, then add 10mL of acetic acid for reaction for 1.5h, wash with clean water until the supernatant does not turn red when tested with pH paper; test the sulfonate ion density to be 1.4-3.6mmol / g; dry the microspheres in a 100℃ oven overnight.
[0095] ④ Repeat the above step ③ twice with the dried microspheres to detect the density of the microspheres after multiple sulfonation.
[0096] ⑤ Take 10 g of sulfonated microspheres, add 2.69 g of ferrous chloride tetrahydrate, 7.31 g of ferric chloride pentahydrate, and 100 mL of water, and stir ultrasonically for 0.5 h.
[0097] ⑥ Heat the solution to 85°C to remove the hydrochloric acid in the solution, cool to room temperature and continue stirring for 2 hours.
[0098] ⑦ Add 20 mL of aqueous ammonia and heat to 85°C for 1 hour.
[0099] (3) Surface coating of magnetic microspheres
[0100] ① Prepare 2.5% PVP K88W (high viscosity stabilizer) ethanol solution, add 10% PVA aqueous solution to make 80% ethanol aqueous solution, pour the magnetized magnetic microspheres into it to make a 1% magnetic microsphere solution, and observe monodispersity under an ultrasonic microscope.
[0101] ② Add 1 times the mass of magnetic microspheres of ammonia water, sonicate until the microspheres are monodisperse, add 4 times the mass of magnetic microspheres of tetraethyl orthosilicate (silane coupling agent), and react at room temperature overnight.
[0102] ③ The magnetic microspheres were centrifuged, washed with 20% ethanol solution until the supernatant was transparent, and dried in a drying oven at 120° C. for 24 h to obtain magnetic microspheres coated with silica.
[0103] (4) Surface functionalization of magnetic microspheres
[0104] ① Take 1g of magnetic microspheres wrapped with silica, add 40g of dimethyl sulfoxide, and ultrasonically disperse for 10 minutes; then, add 90g of dichloroethane to make a 1% magnetic microsphere solution, add 5g of diethylene glycol glycidyl ether and 1g of glycolic acid, and stir to disperse.
[0105] ② After stirring at 0℃ for 30min, add 200uL of boron trifluoride ether and react at 0℃ for 24h.
[0106] ③ After the reaction is completed, the magnetic microspheres are taken out, washed twice with ethanol, and then washed twice with pH 7.0 PBS buffer to obtain the desired hydrophilic monodisperse carboxyl magnetic microspheres.
[0107] Example 3
[0108] A method for preparing hydrophilic monodisperse carboxyl magnetic microspheres of this embodiment comprises the following steps:
[0109] (1) Microsphere template synthesis
[0110] ① Take 100g of deionized water, 1400g of anhydrous ethanol, and 22.5g of pvp K88 (stabilizer) and put them into a 3L three-necked flask and place it in a water bath.
[0111] ②Introduce nitrogen into the three-necked flask, insert a 200℃ thermometer into the three-necked flask, and control the temperature inside the three-necked flask to about 69℃.
[0112] ③ Take 200g of styrene, add 1.5g of AIBN (azobisisobutyronitrile), and stir evenly; after the inside of the three-necked flask is stable, pour the styrene and other mixtures into it and react for 2h (the solution starts to become turbid 12min after adding styrene).
[0113] ④ Take 40g of DVB (divinylbenzene), add 90g of ethanol and 0.1% of mercaptoethanol and mix; after styrene reacts for 3h, drip the crosslinking agent, ethanol and mercapto compound mixture into the three-necked flask at a speed of 10rmp / min through a peristaltic pump, and the dripping will be completed in about 1.5h.
[0114] ⑤ Continue the reaction for 2.5h or until the whole reaction time is 6h, then take out the reaction mixture.
[0115] ⑥ Pour the reaction into a centrifuge bottle, centrifuge at 2000 rpm for 20 min, and discard the supernatant; add ethanol to ultrasonically clean the precipitated microspheres until they are dispersed, centrifuge at 2000 rpm for 10 min, and repeat once; add a small amount of ethanol, mix the microspheres and add them to a single-mouth flask, rotary evaporate the microspheres until they are dry, and put them in a 70°C oven for drying overnight to obtain solid PS-DVB microspheres (1um uniform microspheres observed under an electron microscope, such as Figure 1 shown).
[0116] (2) Microsphere magnetization
[0117] ① Weigh 10 g of dried PS-DVB microspheres, put them into a beaker, add 100 g of dichloroethane, and crush them in an ultrasonic crusher for 20 min (ice bath, 300 W power, on for 2 s and off for 5 s).
[0118] ② After the ultrasonic treatment, pour the solution into a three-necked flask, rinse the beaker with acetic acid, and add acetic acid to the three-necked flask until the total mass of the solution is 160 g (including 10 g of PS-DVB microspheres).
[0119] ③ Place the three-necked flask in an 85℃ oil bath and heat for 2h, then add 5mL of concentrated sulfuric acid and react for 1.5h. Wash with clean water until the supernatant does not turn red when tested with pH paper; test the sulfonate ion density to be 1.4-3.6mmol / g; dry the microspheres in a 100℃ oven overnight.
[0120] ④ Repeat the above step ③ twice with the dried microspheres to detect the density of the microspheres after multiple sulfonation.
[0121] ⑤ Take 10 g of sulfonated microspheres, add 2.69 g of ferrous chloride tetrahydrate, 7.31 g of ferric chloride pentahydrate, and 100 mL of water, and stir ultrasonically for 0.5 h.
[0122] ⑥ Heat the solution to 80°C to remove the hydrochloric acid in the solution, cool to room temperature and continue stirring for 2 hours.
[0123] ⑦ Add 20mL of ammonia water, heat to 80℃ and react for 1h to obtain magnetic microspheres (morphology under electron microscope, as shown in Figure 5). Figure 2 shown).
[0124] (3) Surface coating of magnetic microspheres
[0125] ① Prepare a 2% PVP K88 (high viscosity stabilizer) ethanol solution, add 10% PVA aqueous solution to make an 80% ethanol aqueous solution, pour the magnetized magnetic microspheres into it to make a 1% magnetic microsphere solution, and observe monodispersity under an ultrasonic microscope.
[0126] ② Add 1 times the mass of magnetic microspheres of ammonia water, ultrasonicate until the microspheres are monodisperse, add 3 times the mass of magnetic microspheres of tetraethyl orthosilicate and 1 times the mass of KH550 (silane coupling agent), and react at room temperature overnight.
[0127] ③ The magnetic microspheres were centrifuged, washed with 20% ethanol solution until the supernatant was transparent, and dried in a drying oven at 120°C for 24 h to obtain magnetic microspheres coated with silica (morphology under electron microscope, such as Figure 3 shown).
[0128] (4) Surface functionalization of magnetic microspheres
[0129] ① Take 1g of magnetic microspheres wrapped with silica, add 25g of dimethyl sulfoxide, and ultrasonically disperse for 10 minutes; then, add 75g of dichloroethane to make a 1% magnetic microsphere solution, add 3g of diethylene glycol glycidyl ether and 0.8g of glycolic acid, and stir to disperse.
[0130] ② After stirring at 0℃ for 30min, add 200uL of boron trifluoride ether and react at 0℃ for 24h.
[0131] ③After the reaction is completed, the magnetic microspheres are taken out, washed twice with ethanol, and then washed twice with pH 7.0 PBS buffer to obtain the desired hydrophilic monodisperse carboxyl magnetic microspheres (morphology under electron microscope as shown in Figure 4 , 5 shown).
[0132] Comparative Example 1
[0133] The preparation method of a magnetic microsphere in this comparative example is basically the same as that in Example 3, the main difference is that: in step (1) during the synthesis of the microsphere template, no crosslinking agent - DVB and mercaptoethanol are added.
[0134] Comparative Example 2
[0135] The preparation method of a magnetic microsphere in this comparative example is basically the same as that in Example 3, the main difference is that in step (2) the microsphere magnetization process, the microsphere is sulfonated with different solvents (glacial acetic acid), and the sulfonation treatment is only performed once.
[0136] Comparative Example 3
[0137] The preparation method of a magnetic microsphere in this comparative example is basically the same as that in Example 3, the main difference is that in step (3) during the surface coating of the magnetic microsphere, no high viscosity stabilizer (PVP K88) is added.
[0138] Comparative Example 4
[0139] The preparation method of a magnetic microsphere in this comparative example is basically the same as that in Example 3, the main difference is that in step (4) functionalization of the surface of the magnetic microsphere, a layer of carboxyl groups is directly modified on the surface of the magnetic microsphere coated with silica without polymer coating.
[0140] Experimental Example 1
[0141] This experimental example is used to verify the effect of adding "crosslinking agent-DVB and mercaptoethanol" on the synthesis of microsphere templates.
[0142] 1. Experimental methods:
[0143] The corresponding microsphere templates were prepared by the method of the present invention (taking Example 3 as an example) and the method of Comparative Example 1, respectively, and the rigidity and integrity of the two microspheres in a non-polar solution were tested.
[0144] 2. Experimental results:
[0145] The results are as follows Figure 6 As shown. Figure 6 It can be seen that the uncrosslinked polystyrene microspheres ( Figure 6 A) in a non-polar solvent, after centrifugation, the microspheres are deformed; while the cross-linked microspheres of the present invention ( Figure 6 B) Under the same conditions, it can still maintain a complete rigid structure.
[0146] The above results show that by adding a certain amount of crosslinking agent and mercaptoethanol during the polymerization process, the present invention can prepare solid crosslinked polystyrene microspheres, which can maintain rigidity in non-polar solutions and maintain a certain integrity under many extreme conditions such as centrifugation.
[0147] Experimental Example 2
[0148] This experimental example is used to verify the effect of sulfonation times and sulfonation reagents on the magnetization results of microspheres.
[0149] 1. Experimental methods:
[0150] According to the method of the present invention (taking Example 3 as an example), corresponding magnetic microspheres with different sulfonation times were prepared. At the same time, magnetic microspheres were also prepared according to the method of Comparative Example 2, and the sulfonation density and magnetic response speed of the four kinds of magnetic microspheres were tested in batches.
[0151] 2. Experimental results:
[0152] The results are shown in Table 1.
[0153] Table 1 Effect of different sulfonation methods on the magnetization of microspheres
[0154]
[0155] From the above results, it can be seen that multiple sulfonation of the microspheres can enable the microspheres to adsorb more ferric ions and ferrous ions, fix more magnetic particles on the microspheres in a more stable form, and enhance their magnetic response speed; at the same time, the selection of the sulfonation reagent of the present invention can maximize the sulfonation efficiency.
[0156] Experimental Example 3
[0157] This experimental example is used to verify the effect of adding a "high viscosity stabilizer" on the surface coating of magnetic microspheres.
[0158] 1. Experimental methods:
[0159] The corresponding magnetic microspheres coated with silica were prepared by the method of the present invention (taking Example 3 as an example) and the method of Comparative Example 3, respectively, and the morphology of the microspheres was observed.
[0160] 2. Experimental results:
[0161] Without the addition of high viscosity stabilizer (PVP K88), the magnetic beads can be seen to aggregate with the naked eye, and the sedimentation rate at a height of 1 cm is within 10 minutes. However, with the addition of high viscosity stabilizer (PVP K88), the magnetic beads are evenly dispersed under a microscope, and the sedimentation rate at a height of 1 cm is controlled to be more than 2 hours.
[0162] From the above results, it can be seen that the addition of a high viscosity stabilizer (PVP K88) during the silicon coating process of the present invention can reduce the speed of silica gel cross-linking, and at the same time, the magnetic particles are dispersed in the high viscosity stabilizer by ultrasound to form monodisperse magnetic beads, and finally a high temperature treatment is performed to further cross-link the residual silanol groups on the surface to prevent the magnetic particles from falling off.
[0163] Experimental Example 4
[0164] This experimental example is used to verify the effect of the "magnetic microsphere surface functionalization" method of the present invention on the performance of carboxyl magnetic microspheres.
[0165] 1. Experimental methods:
[0166] The corresponding carboxyl magnetic microspheres were prepared by the method of the present invention (taking Example 3 as an example) and the method of Comparative Example 4, and the carboxyl density thereof was measured.
[0167] 2. Experimental results:
[0168] The results are shown in Table 2.
[0169] Table 2 Effect of “magnetic microsphere surface functionalization” on the performance of carboxyl magnetic microspheres
[0170]
[0171]
[0172] From the above results, it can be seen that the invention coats a layer of polymer on the basis of silica gel and modifies a layer of carboxyl groups on the surface of the polymer, which can significantly increase the carboxyl density of the microspheres (reflecting hydrophilicity) and make the functional groups on the surface of the microspheres rich and not easy to fall off.
[0173] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing hydrophilic monodisperse carboxyl magnetic microspheres, characterized in that: The steps include: (1) Microsphere template synthesis Monodisperse microsphere templates were prepared by dispersion polymerization, and solid polystyrene microspheres were obtained by adding a cross-linking agent during the polymerization process. (2) Microsphere magnetization The surface of the microspheres is sulfonated to make the microspheres negatively charged; then the negatively charged microspheres are used to adsorb positively charged iron ions and ferrous ions to complete the magnetization of the microspheres; (3) Surface coating of magnetic microspheres The surface of the magnetic microspheres is coated with silicon dioxide, and then solidified to obtain magnetic microspheres coated with silicon dioxide; (4) Surface functionalization of magnetic microspheres After the surface of the magnetic microspheres wrapped with silica is coated with polymer, the surface is then modified with carboxyl groups.
2. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 1, characterized in that: In the step (1), the specific process of synthesizing the microsphere template is as follows: ①Put deionized water, anhydrous ethanol and stabilizer into a three-necked flask and place it in a water bath; ②Introduce nitrogen into the three-necked flask and control the temperature inside the three-necked flask to 68-70°C; ③Take styrene, add azobisisobutyronitrile, stir evenly; pour the mixture into a three-necked flask and react; ④ Take the cross-linking agent, add ethanol and thiol compound to mix; after styrene reacts for 2 to 4 hours, drip the cross-linking agent, ethanol and thiol compound mixture into the three-necked flask through a peristaltic pump; ⑤Continue the reaction until the entire reaction is completed; ⑥ Pour the reactants into a centrifuge bottle, centrifuge and discard the supernatant; add ethanol to ultrasonically clean the precipitated microspheres until they are dispersed, centrifuge, and repeat once; add ethanol, mix the microspheres and add them to a single-necked flask; rotary evaporate the microspheres until dry, and put them in an oven to dry overnight to obtain the solid polystyrene microspheres required for the target.
3. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 2, characterized in that: The stabilizer selected is pvp K88.
4. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 2, characterized in that: The crosslinking agent is selected from one or more of divinylbenzene and ethylene glycol dimethacrylate.
5. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 2, characterized in that: The particle size of the prepared polystyrene microspheres is 1 um.
6. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 1, characterized in that: In the step (2), the specific process of microsphere magnetization is as follows: ① Weigh the dried polystyrene microspheres, put them into a beaker, add acetic acid or ethylene dichloride, and crush them in an ultrasonic crusher; ②After the ultrasound is completed, pour the solution into a three-necked flask, rinse the beaker with acetic acid, and add it to the three-necked flask; ③ Place the three-necked flask in an oil bath at 70-100℃ and heat it, then add concentrated sulfuric acid or acetic acid to react, wash with clean water until the supernatant does not turn red when tested with pH paper; test the sulfonate ion density to be 1.4-3.6mmol / g; put the microspheres in an oven to dry; ④ Repeat the above step ③ several times with the dried microspheres to detect the density of the microspheres after multiple sulfonation; ⑤ Take the sulfonated microspheres, add ferrous chloride tetrahydrate, ferric chloride pentahydrate and water, mix, and stir with ultrasound; ⑥ Heat the solution to 75-85°C to remove the hydrochloric acid in the solution, cool it to room temperature and continue stirring; ⑦ Add ammonia water and heat to 75-85℃ for reaction.
7. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 6, characterized in that: In the step (2)⑤, 10 g of sulfonated microspheres, 2.69 g of ferrous chloride tetrahydrate, 7.31 g of ferric chloride pentahydrate, and 100 mL of water.
8. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 1, characterized in that: In the step (3), the specific process of coating the surface of the magnetic microspheres is as follows: ① Prepare an ethanol solution containing PVP K88, add PVA aqueous solution to prepare an 80% ethanol aqueous solution; pour the magnetized microspheres into the 80% ethanol aqueous solution to obtain a magnetic microsphere solution; ② Add ammonia water, sonicate until the microspheres are monodispersed, add silane coupling agent, and react overnight at room temperature; ③ Centrifuge the magnetic microspheres, wash with ethanol solution until the supernatant is transparent, and dry them in a drying oven to obtain magnetic microspheres coated with silica.
9. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 8, characterized in that: The silane coupling agent is selected from one or more of tetraethyl orthosilicate, KH550, and trimethylchlorosilane.
10. The method for preparing hydrophilic monodisperse carboxyl magnetic microspheres according to claim 1, characterized in that: In the step (4), the specific process of functionalizing the surface of the magnetic microspheres is as follows: ① Take the magnetic microspheres wrapped with silica, add dimethyl sulfoxide, and disperse them by ultrasonication; then, add ethylene dichloride to prepare a magnetic microsphere solution, add diethylene glycol glycidyl ether and glycolic acid, and stir and disperse; ② Add boron trifluoride etherate and react; ③ After the reaction is completed, the magnetic microspheres are taken out, washed with ethanol, and then washed with PBS buffer to obtain the desired hydrophilic monodisperse carboxyl magnetic microspheres.
Citation Information
Cited By
Novel chemiluminescence immunomagnetic bead as well as preparation process and application thereof