Preparation method of flame-retardant reinforced nylon 6 composite material and composite material prepared from flame-retardant reinforced nylon 6 composite material

By adding flame retardant during the hydrolysis and polymerization of caprolactam and mixing it with glass fibers, a flame retardant reinforced nylon 6 composite material was prepared by a one-step melting process, which solved the molecular chain oxidation problem caused by multiple melting, significantly improving the mechanical strength of the material and Flame retardant effect.

CN118930910APending Publication Date: 2024-11-12DONGMING RISUN CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411184323.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When preparing flame retardant reinforced nylon 6 composite materials in the prior art, multiple polymerization/melting processes are required to cause chain oxidation, yellowing, and chain breakage of nylon 6 molecules, affecting the mechanical strength of the material.

Method used

The flame retardant is added during the hydrolysis polymerization of caprolactam, and the polymer melt is mixed with glass fiber at the outlet of the polymerization kettle. The flame retardant reinforced nylon 6 composite material is prepared through a one-step melting process, reducing the melting of the nylon 6 modification process frequency.

Benefits of technology

It effectively improves the mechanical strength of the material, increases the tensile strength by 1.2 to 1.4 times, reduces energy consumption, and retains the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930910A_ABST
    Figure CN118930910A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a flame-retardant reinforced nylon 6 composite material, the flame-retardant reinforced nylon 6 composite material prepared from the flame-retardant reinforced nylon 6 composite material, a preparation method of a flame-retardant reinforced nylon 6 composite material component and the flame-retardant reinforced nylon 6 composite material component prepared from the flame-retardant reinforced nylon 6 composite material component. According to the invention, the melting frequency of nylon 6 is reduced, the mechanical properties of the material are effectively retained, the tensile strength is improved by 1.2-1.4 times compared with that of the traditional post-modification process, and the energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of composite materials, and in particular to a method for preparing a flame retardant reinforced nylon 6 composite material. Background Art

[0002] Flame retardant reinforced nylon 6 is a high-strength, flame-retardant polymer composite material. Its strength is improved by adding glass fiber, carbon fiber or other organic / inorganic fibers; the flame retardant property is achieved by adding inorganic or organic flame retardants. With the enhancement of people's environmental awareness, halogen-free flame retardants are gradually replacing halogenated flame retardants and becoming the mainstream.

[0003] When the glass fiber content of flame retardant reinforced nylon 6 is 25-30%, the tensile strength can reach 110-150MPa, and the flame retardant grade reaches V0 (0.8mm). It is widely used as engineering plastics in the fields of electronics, rail transportation, machinery, etc. With the widespread popularity of new energy vehicles, flame retardant reinforced nylon 6 materials can be used as battery modules, charging system components, high-voltage connectors, charging piles, thermal management system components, etc. The demand for flame retardant nylon 6 for new energy vehicle battery modules alone reaches 360,000 tons / year.

[0004] At present, the most commonly used method for preparing flame-retardant reinforced nylon 6 is melt blending, in which nylon 6, flame retardant, and glass fiber are added to a twin-screw extruder to prepare flame-retardant nylon by physical blending. However, when preparing flame-retardant reinforced nylon by this method, it is necessary to first synthesize nylon 6 from caprolactam polymerization, and then prepare flame-retardant reinforced nylon 6 through twin-screw melt blending. During molding, it is also necessary to melt the screw of the injection molding machine again, that is, it takes three polymerization / melting processes to transform pure nylon 6 into flame-retardant reinforced nylon 6 parts. After each melting, the nylon 6 molecular chain will be oxidized, yellowing will occur, and the molecular chain will break, resulting in a decrease in mechanical strength, which affects the practical application of nylon 6 composite materials.

[0005] Patent CN202211526093.2, patent CN202211513234.7, patent CN202211525019.9, and patent CN202210271086.6 each disclose a method for preparing flame-retardant reinforced nylon composite materials. These methods all adopt a post-modification method, that is, nylon 6, flame retardant and glass fiber are modified by melt blending, which increases the melting times of the nylon composite material, resulting in oxidation, yellowing, and chain breakage of the nylon 6 molecular chain, which reduces the mechanical strength of the material. Summary of the invention

[0006] Therefore, in view of the problems existing in the flame retardant and reinforced modification technology of nylon 6 in the prior art, the applicant found that a flame retardant was added during the hydrolysis and polymerization of caprolactam, and the polymer melt was mixed with glass fiber in an impregnation mold at the outlet of the polymerization kettle, followed by pelletizing, extraction, and drying. A flame retardant and reinforced nylon 6 composite material was prepared through a one-step melting process, which can reduce the number of melting times in the nylon 6 modification process and improve the mechanical strength of the material. The present invention was completed on this basis.

[0007] According to one aspect of the present invention, a method for preparing a flame retardant reinforced nylon 6 composite material is provided, the method comprising the following steps:

[0008] (S1) caprolactam, a flame retardant and deionized water are mixed in a weight ratio of (50-100):(5-10):1, reacted for 4-6 hours under an inert atmosphere at a temperature of 240-265° C. and a pressure of 0.3-0.7 MPa, then the temperature is reduced to 230-240° C., and the pressure is reduced to below 100 Pa, and the reaction is continued for 1-3 hours to obtain a polymer product;

[0009] (S2) preheating the glass fiber to 110-250° C. and then introducing the glass fiber into an impregnation mold, and introducing the polymer product of step (S1) into the impregnation mold through another feed port, so that the glass fiber is impregnated with the polymer product prepared in step (S1), so as to obtain a glass fiber impregnated with the polymer product;

[0010] (S3) Cooling and granulating the glass fiber impregnated with the polymerization product prepared in step (S2), and then extracting and drying to obtain a flame retardant reinforced nylon 6 composite material.

[0011] According to one embodiment of the present invention,

[0012] The glass fiber is spooled glass fiber.

[0013] According to one embodiment of the present invention,

[0014] In step (S1), the flame retardant is 6,6'-(1-phenylethane-1,2-diyl)bis(dibenzo[c,e][1,2]-phosphine-6-oxide), namely PHED.

[0015] According to one embodiment of the present invention,

[0016] In step (S1), the inert atmosphere refers to a nitrogen atmosphere or an argon atmosphere.

[0017] According to one embodiment of the present invention,

[0018] In step (S2), the impregnation mold includes 3-7 tension wheels, or includes an inclined channel with a changing direction.

[0019] Through the action of the tensioning wheel or the inclined channel with changing direction, the glass fiber bundle can be simply dispersed into individual glass fibers to facilitate the simultaneous impregnation process.

[0020] According to one embodiment of the present invention,

[0021] In step (S2), the feed ratio of the glass fiber to the caprolactam used in step (S1) is 0.2:1 to 0.4:1 by weight.

[0022] According to one embodiment of the present invention,

[0023] In step (S2), the temperature in the dipping mold is 200-270°C.

[0024] According to one embodiment of the present invention,

[0025] In step (S3), the cooling refers to cooling at 30-70°C.

[0026] According to another aspect of the present invention, a flame retardant reinforced nylon 6 composite material is provided, which is prepared by the above method.

[0027] According to another aspect of the present invention, there is provided a method for preparing a flame retardant reinforced nylon 6 composite material component, the method comprising:

[0028] (S4) molding the flame retardant reinforced nylon 6 composite material at 230-260° C. to obtain a flame retardant reinforced nylon 6 composite material component.

[0029] According to another aspect of the present invention, a flame retardant reinforced nylon 6 composite material component is provided, which is prepared by the above method.

[0030] Beneficial Effects

[0031] The present invention synthesizes a flame-retardant reinforced nylon 6 composite material in a polymerization reactor in one step, and then obtains a flame-retardant nylon 6 component through a single injection molding process. Compared with the traditional nylon 6 post-modification process, the present invention reduces the number of melting times of nylon 6, effectively retains the mechanical properties of the material, and improves the tensile strength by 1.2 to 1.4 times compared with the traditional post-modification process, and reduces energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of synthesizing a flame retardant reinforced nylon 6 composite material according to one embodiment of the present invention.

[0033] Figure 2 It is a schematic diagram of synthesizing a flame retardant reinforced nylon 6 composite material according to another embodiment of the present invention. DETAILED DESCRIPTION

[0034] In order to enable persons with ordinary knowledge in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and the scope of the patent application. Unless otherwise specified, all technical and scientific words used in the text have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.

[0035] In the present invention, the caprolactam used was purchased from Dongming Xuyang Chemical Co., Ltd., the flame retardant PHED was purchased from Hubei Jiahui Xingcheng Biotechnology Co., Ltd., the universal material testing machine and impact testing machine were purchased from Jinan Fangyuan Testing Instrument Co., Ltd., the vertical combustion tester was purchased from Shanghai Farui Instrument Technology Co., Ltd., and the injection molding machine was purchased from Suzhou Dewino Machinery Equipment Co., Ltd.

[0036] Example

[0037] Comparative Example 1:

[0038] Weigh 700g of nylon 6 resin, 70g of PHED flame retardant, and 2.1g of 1010 antioxidant, mix them in a high-speed mixer for 30 minutes, and then put them into the hopper of a twin-screw extruder. The extrusion temperature is 210-260°C. Use spooled glass fiber, the amount is 30% of nylon 6 resin, add it to the glass fiber adding hole of the twin-screw extruder, and after water cooling, pelletizing, extraction, and drying, obtain a flame-retardant reinforced nylon 6 composite material. The flame-retardant nylon 6 particles are injection molded into tensile, impact and flame-retardant specimens at 240-260°C, and their mechanical and flame-retardant properties are tested.

[0039] Comparative Example 2:

[0040] A flame retardant reinforced nylon 6 composite material was prepared in the same manner as in Example 1, except that short fibers were used as glass fibers and added to the side feed hole using a side feeder.

[0041] Embodiment 1:

[0042] Weigh 700g of caprolactam, 70g of PHED flame retardant, and 10g of deionized water, add them into the polymerization kettle, replace with nitrogen 3 times, raise the temperature of the polymerization kettle to 260℃, pressure 0.5MPa, and react for 5h. Then lower the temperature to 235℃, release the pressure, evacuate to 100Pa, react for 2h, discharge the product from the reactor, and enter Figure 1In the impregnation mold shown, it is mixed with spool glass fiber (spool glass fiber has been preheated at 230°C and the amount is 30% of caprolactam), and the temperature in the mold is maintained at 250°C. Then it is water-cooled at 50°C, pelletized, extracted, and dried to obtain flame-retardant reinforced nylon 6. The flame-retardant nylon 6 particles are injection molded into tensile, impact and flame-retardant specimens at 240-260°C to test their mechanical and flame-retardant properties.

[0043] Embodiment 2:

[0044] Weigh 700g of caprolactam, 70g of PHED flame retardant, and 10g of deionized water, add them into the polymerization kettle, replace with nitrogen 3 times, raise the temperature of the polymerization kettle to 260℃, pressure 0.5MPa, and react for 5h. Then lower the temperature to 235℃, release the pressure, evacuate to 100Pa, react for 2h, discharge the product from the reactor, and enter Figure 2 In the impregnation mold shown, it is mixed with spool glass fiber (spool glass fiber has been preheated at 200°C and the amount is 30% of caprolactam), and the temperature in the mold is maintained at 260°C. Then it is water-cooled at 40°C, pelletized, extracted, and dried to obtain flame-retardant reinforced nylon 6. The flame-retardant nylon 6 particles are injection molded into tensile, impact and flame-retardant specimens at 240-260°C to test their mechanical and flame-retardant properties.

[0045] Experimental Example 1:

[0046] The following tests were performed on pure nylon 6, the above-mentioned comparative examples 1-2 and examples 1-2:

[0047] Tensile strength: measured according to ISO 527-1 / -2 method;

[0048] Elongation at break: measured according to ISO 527-1 / -2 method;

[0049] Notched impact strength: measured according to ISO 179 / 1eA method;

[0050] LOI: measured according to GB / T2406-1992 method;

[0051] Flame retardant grade: measured according to GB2409-84 method;

[0052] The above measurement results are listed in the following table 1

[0053] Table 1 Test results of embodiments and comparative examples

[0054]

[0055] From the above table, it can be seen that in Comparative Examples 1 and 2, nylon 6 is flame-retarded and reinforced by melt blending, and then the strips are obtained by injection molding. In addition to polymerization, the strips undergo two melting processes (twin-screw extrusion and injection molding). The tensile strength, elongation at break, and notched impact strength of the obtained strips are 125.4 MPa, 112.4 MPa, 4%, 3.8%, and 3.5 kJ / m, respectively. 2 、3.4kJ / m 2 The reinforcing effect of short fibers is lower than that of spooled glass fibers, which is related to the short retention length of glass fibers in nylon 6. In Examples 1 and 2 of the present application, a flame-retardant reinforced nylon 6 composite material is prepared in one step in a polymerization reactor. After a single injection molding melting process, the obtained strip tensile strength, elongation at break, and notched impact strength are higher than those of Comparative Examples 1 and 2, with Example 2 having the best result. The above results show that reducing the number of nylon 6 melting times can effectively retain the mechanical properties of the material and have a better flame retardant effect.

Claims

1. A method for preparing a flame retardant reinforced nylon 6 composite material, the method comprising the following steps: (S1) caprolactam, a flame retardant and deionized water are mixed in a weight ratio of (50-100):(5-10):1, reacted for 4-6 hours under an inert atmosphere at a temperature of 240-265° C. and a pressure of 0.3-0.7 MPa, then the temperature is reduced to 230-240° C., and the pressure is reduced to below 100 Pa, and the reaction is continued for 1-3 hours to obtain a polymer product; (S2) preheating the glass fiber to 110-250° C. and then introducing the glass fiber into an impregnation mold, and introducing the polymer product of step (S1) into the impregnation mold through another feed port, so that the glass fiber is impregnated with the polymer product prepared in step (S1), so as to obtain a glass fiber impregnated with the polymer product; (S3) Cooling and granulating the glass fiber impregnated with the polymerization product prepared in step (S2), and then extracting and drying to obtain a flame retardant reinforced nylon 6 composite material.

2. The method according to claim 1, wherein In step (S1), the flame retardant is 6,6'-(1-phenylethane-1,2-diyl)bis(dibenzo[c,e][1,2]-phosphine oxide-6-oxide).

3. The method according to claim 1, wherein In step (S1), the inert atmosphere refers to a nitrogen atmosphere or an argon atmosphere.

4. The method according to claim 1, wherein In step (S2), the impregnation mold includes 3-7 tension wheels, or includes an inclined channel with a changing direction.

5. The method according to claim 1, wherein In step (S2), the feed ratio of the glass fiber to the caprolactam used in step (S1) is 0.2:1 to 0.4:1 by weight.

6. The method according to claim 1, wherein In step (S2), the temperature in the dipping mold is 200-270°C.

7. The method according to claim 1, wherein In step (S3), the cooling refers to cooling at 30-70°C.

8. A flame retardant reinforced nylon 6 composite material, prepared according to the method according to any one of claims 1 to 7.

9. A method for preparing a flame retardant reinforced nylon 6 composite material component, the method comprising: (S4) Molding the flame retardant reinforced nylon 6 composite material according to claim 8 at 230-260° C. to obtain a flame retardant reinforced nylon 6 composite material component.

10. A flame retardant reinforced nylon 6 composite material component, prepared according to the method according to claim 9.

Citation Information

Patent Citations

  • Halogen-free flame-retardant glass fiber reinforced nylon as well as preparation method and application thereof

    CN114479446A

  • Halogen-free intumescent flame-retardant material as well as preparation method and application thereof

    CN115746559A

  • Preparation method of nylon 6 flame-retardant composite material

    CN115819961A

  • Efficient halogen-free flame retardant method for nylon 6 glass fiber reinforced material

    CN115895247A