Hardening protective film capable of prolonging service life of folding mobile phone and preparation method of hardening protective film
By using the laminated substrate, hardened coating and fluorine-containing protective film on the folding mobile phone, the problem of cracking of the folding mobile phone protective film is solved, improving service life and wear resistance, and improving user experience.
Patent Information
- Application Number
- CN202411014428.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
During the use of the folding mobile phone, cracks and wear are prone to bending areas of the protective film, resulting in a shortened service life, increasing replacement costs, and reducing consumer experience.
The substrate, hardened coating and fluorine-containing layer are laminated in sequence. The hardened coating is composed of polyurethane acrylic resin and surface-modified nanosilica particles. The fluorine-containing layer is a perfluoropolyether silicone resin. Improve wear resistance by optimizing formulation and stacked structure.
It significantly improves the service life of the folding phone, reduces wear and cracks after bending, and improves the wear resistance and user experience of the protective film.
Smart Images

Figure CN118930937A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of mobile phone protective film materials, and in particular to a hardened protective film capable of prolonging the service life of a foldable mobile phone and a preparation method thereof. Background Art
[0002] In recent years, with the development of foldable smartphones, more and more consumers are using foldable phones. Foldable phones have brought consumers a fresh user experience and various practical conveniences. However, with the increase in the number of consumer groups and people using foldable phones, various usage situations may arise. For example, the screen of a foldable phone may touch the surfaces of various objects, such as wooden desktops, marble desktops, plastic desktops, jeans, artificial nails, other mobile phones, notebooks, etc. In order to protect the screen of a foldable phone, a hard-coated protective film is usually affixed to the screen of the foldable phone. Although the service life of the mobile phone screen is further improved, during the contact process, the surface of the hardened protective film of various objects will also cause certain slight wear or even severe wear, especially the bending area of the hardened protective film on the surface of the object causes certain wear. With the increase in the number of bending times and after bending in high temperature, low temperature, high temperature and high humidity scenes, the protective film in the folding area will have certain cracks, causing the protective film to fail, greatly reducing the service life of the hardened protective film, increasing the cost of replacing the protective film, reducing the consumer's user experience, and even reducing consumers' confidence in foldable phones.
[0003] As mentioned above, in various usage scenarios, the foldable mobile phone screen may touch or rub against various objects, causing certain wear on the surface of the protective film on the mobile phone screen. When observed at a microscopic level, microscopic defects may appear on the surface of the hardened protective film (see Figure 1 ), under the condition of continuous bending, due to the effect of bending stress, the microscopic defects will be further amplified and extended, and even directly cause cracks in the hard coating.
[0004] Therefore, it is necessary to improve the existing technology to provide a more reliable solution. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a hardened protective film and a preparation method thereof that can increase the service life of a foldable mobile phone in view of the deficiencies in the above-mentioned prior art.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows: In a first aspect of the present invention, a hardened protective film capable of improving the service life of a foldable mobile phone is provided, comprising a substrate, a hardened coating layer and a fluorine-containing layer stacked in sequence;
[0007] Wherein, the hardened coating is obtained by coating hardened glue and then curing, and the fluorine-containing layer is obtained by coating AF coating liquid and then curing;
[0008] The hardened glue is a mixture of polyurethane acrylic resin and inorganic particles, and the inorganic particles contain hydroxyl groups and organic siloxane introduced by surface modification;
[0009] The AF coating liquid is a perfluoropolyether siloxane resin solution.
[0010] Preferably, the molar ratio of the hydroxyl group on the surface of the inorganic particles to the organosiloxane is 8:2 to 5:5.
[0011] Preferably, the mass percentage of inorganic particles in the hardened glue is 30% to 50%.
[0012] The inorganic particles are nano-silicon dioxide with a particle size of 10 to 30 nm and surface-modified with organic siloxane.
[0013] Preferably, the organosiloxane is 3-(methacryloyloxy)propyltrimethoxysilane.
[0014] Preferably, the surface-modified nano-silica with organosiloxane is prepared by the following method:
[0015] S1-1. At 25°C, 2.5-10 mL of a mixture of Triton X-100 and n-octanol was mixed with 1.5-6 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.45-1.8 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0016] Under stirring, 1.5-6 mL of ethyl orthosilicate is added dropwise, stirring is continued for 1.5-6 hours, centrifuged and filtered, and the obtained nano-silicon dioxide is dispersed with anhydrous ethanol to a nano-silicon dioxide dispersion with a solid content of 10-30%. The hydroxyl content on the surface of the obtained nano-silicon dioxide is measured.
[0017] S1-2, take 10-40 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 3-(isomethacryloyloxy)propyltrimethoxysilane, control the molar ratio of hydroxyl groups on the surface of the nano-silica to 3-(isomethacryloyloxy)propyltrimethoxysilane to be 8:2-5:5, stir the reaction at 50°C for 5-20 hours, centrifuge at 5000-20000 rpm for 0.5-2 hours, and after solid precipitation, wash and centrifuge for multiple times to obtain nano-silica with surface modified organic siloxane.
[0018] Preferably, the weight average molecular weight of the perfluoropolyether siloxane resin is 5000-10000, and the molecular structure is shown in Formula 1 below:
[0019]
[0020] The value range of n is 24-52.
[0021] Preferably, the solid content of the AF coating liquid is 5-20%.
[0022] Preferably, the AF coating solution is prepared by the following method:
[0023] S2-1, weigh 50g of perfluoropolyether acyl fluoride into a reaction kettle, add 100ml of anhydrous methanol, heat to 50°C and react for 2 hours. The whole process is carried out under 1.5 times the atmospheric pressure and nitrogen protection. Finally, add distilled water for washing until the upper layer is neutral, add dichloromethane and perfluorocyclic ether, separate the liquids, filter, and distill under reduced pressure to obtain perfluoropolyether methyl ester;
[0024] Weigh 20 g of the perfluoropolyether methyl ester prepared in step S2-1, then add 20 g of KH550, react at 60° C. under nitrogen protection for 8 hours, add anhydrous ethanol and perfluorocyclohexane after the reaction, separate the liquids, filter, and perform reduced pressure distillation to obtain a perfluoropolyether aminosiloxane resin, which is then diluted with a perfluoroheptane solvent to a solid content of 5-20% to obtain the AF coating solution.
[0025] Preferably, the thickness of the hardened coating is 3-5 μm; the thickness of the fluorine-containing coating is 7-25 nm, and the dynamic friction coefficient of the surface of the fluorine-containing coating is ≤0.05.
[0026] A second aspect of the present invention provides a method for preparing a hardened protective film capable of prolonging the service life of a foldable mobile phone as described above, characterized in that the method comprises the following steps:
[0027] 1) The hardened glue is evenly coated on the surface of the substrate, and hardened after heat drying and UV curing to obtain a semi-finished product;
[0028] 2) The AF coating liquid is evenly coated on the semi-finished product, and dried at 140-160° C. for 3-8 minutes to obtain the hardened protective film capable of prolonging the service life of the foldable mobile phone.
[0029] The beneficial effects of the present invention are:
[0030] The present invention provides a hardened protective film capable of improving the service life of a foldable mobile phone and a preparation method thereof. The present invention can help improve the wear or damage of the hardened coating during steel wool wear resistance and eraser wear resistance tests by optimizing the formula, designing the laminated structure, and providing the hardened coating and the fluorine-containing coating, thereby reducing the bending failure after wear resistance and further improving the bending life.
[0031] The inorganic particles in the hardening coating are silica particles. Since the refractive index of silica is 1.45-1.47 and the refractive index of the hardening coating is 1.45-1.5, the difference in refractive index between the two is very small, and the rainbow pattern of the hardened film is better. The content of inorganic particles is 30% or 50%. If the content is too low, the hydroxyl groups on the surface of the particles are low, and the number of combinations between methacryloxypropyltrimethoxysilane and inorganic particles is small, which reduces the wear resistance of the hardened film and the wear resistance of the hardened film surface. If the content is too high, the cross-linking performance of the hardening coating itself is reduced, which will also reduce the wear resistance of the hardened film surface.
[0032] The ratio between the hydroxyl group (-OH) on the surface of the inorganic particles and the surface-modified organic siloxane is preferably 8 / 2 or 5 / 5. The surface-modified organic siloxane of the inorganic particles is methacryloxypropyltrimethoxysilane, and the fluorine-containing layer is a fluororesin material containing silanol groups. The molecular structure of the fluororesin is (CF 3 )3-C-CH 2 -CH 2 -CH 2 -C-(Si-OH) 3 When the ratio of hydroxyl groups (-OH) on the surface of inorganic particles to the surface-modified organosiloxane is too high, it is not conducive to the "anchoring" of the inorganic particles in the hardened coating. This is mainly because methacryloxypropyltrimethoxysilane contains unsaturated carbon-carbon double bonds. The hardened coating can undergo a cross-linking reaction with the unsaturated carbon-carbon double bonds contained in methacryloxypropyltrimethoxysilane during UV curing, so it can fix the inorganic nanoparticles well. If there are fewer hydroxyl groups (-OH) on the surface of the inorganic particles, it is not conducive to the chemical combination of the fluorine-containing resin and the particles, thereby reducing the wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a picture of the microscopic defects on the surface of a conventional mobile phone screen protective film. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.
[0035] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.
[0036] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.
[0037] The present invention provides a hardened protective film capable of prolonging the service life of a foldable mobile phone, comprising a substrate, a hardened coating layer and a fluorine-containing layer stacked in sequence;
[0038] The hardened coating is obtained by coating a hardened glue and then curing it, and the fluorine-containing layer is obtained by coating an AF coating liquid and then curing it.
[0039] The hardening glue is a mixture of polyurethane acrylic resin and inorganic particles, and the inorganic particles contain hydroxyl groups (-OH) and organic siloxane introduced by surface modification;
[0040] In a preferred embodiment, the molar ratio of the hydroxyl groups on the surface of the inorganic particles to the organic siloxane is 8:2 to 5:5. More preferably, the ratio is 8:2 or 5:5.
[0041] In a preferred embodiment, the mass percentage of inorganic particles in the hardened glue is 30% to 50%, more preferably 30% or 50%.
[0042] In a preferred embodiment, the inorganic particles are nano-silicon dioxide with a particle size of 10 to 30 nm and a surface modified organic siloxane, and more preferably, the particle size is 10 nm, 20 nm or 30 nm.
[0043] In a preferred embodiment, the organosiloxane is 3-(methacryloyloxy)propyltrimethoxysilane.
[0044] In a preferred embodiment, the surface-modified nano-silica with organic siloxane is prepared by the following method:
[0045] S1-1. At 25°C, 2.5-10 mL of a mixture of Triton X-100 and n-octanol was mixed with 1.5-6 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.45-1.8 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0046] Under stirring, 1.5-6 mL of ethyl orthosilicate is added dropwise, stirring is continued for 1.5-6 hours, centrifuged and filtered, and the obtained nano-silicon dioxide is dispersed with anhydrous ethanol to a nano-silicon dioxide dispersion with a solid content of 10-30%. The hydroxyl content on the surface of the obtained nano-silicon dioxide is measured.
[0047] S1-2, take 10-40 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 3-(isomethacryloyloxy)propyltrimethoxysilane, control the molar ratio of hydroxyl groups on the surface of the nano-silica to 3-(isomethacryloyloxy)propyltrimethoxysilane to be 8:2-5:5, stir the reaction at 50°C for 5-20 hours, centrifuge at 5000-20000 rpm for 0.5-2 hours, and after solid precipitation, wash and centrifuge for multiple times to obtain nano-silica with surface modified organic siloxane.
[0048] In a preferred embodiment, the hardened coating has a thickness of 3-5 μm.
[0049] In a preferred embodiment, the AF coating liquid is a perfluoropolyether siloxane resin solution.
[0050] In a preferred embodiment, the weight average molecular weight of the perfluoropolyether siloxane resin is 5000-10000, and the molecular structure is shown in Formula 1 below:
[0051]
[0052] The value range of n is 24-52.
[0053] In a preferred embodiment, the solid content of the AF coating liquid is 5-20%.
[0054] The thickness of the fluorine-containing coating is 7-25 nm, and the dynamic friction coefficient of the surface of the fluorine-containing coating is ≤0.05.
[0055] In a preferred embodiment, the AF coating solution is prepared by the following method:
[0056] S2-1, weigh 50g of perfluoropolyether acyl fluoride into a reaction kettle, add 100ml of anhydrous methanol, heat to 50°C and react for 2 hours. The whole process is carried out under 1.5 times the atmospheric pressure and nitrogen protection. Finally, add distilled water for washing until the upper layer is neutral, add dichloromethane and perfluorocyclic ether, separate the liquids, filter, and distill under reduced pressure to obtain perfluoropolyether methyl ester;
[0057] Weigh 20 g of the perfluoropolyether methyl ester prepared in step S2-1, then add 20 g of KH550, react at 60 ° C for 8 hours under nitrogen protection, add anhydrous ethanol and perfluorocyclohexane after the reaction, separate the liquids, filter, and distill under reduced pressure to obtain perfluoropolyether aminosiloxane resin, and then dilute with perfluoroheptane solvent to a solid content of 5-20% to obtain AF coating liquid.
[0058] In a preferred embodiment, the substrate thickness is 50 microns of Toray U483, 65 microns of Toray XF7LA7, 75 microns of Toray U483, or 80 microns of Toyobo's SRF.
[0059] The present invention also provides a method for preparing the hardened protective film as above which can prolong the service life of a foldable mobile phone, comprising the following steps:
[0060] 1) The hardened glue is evenly coated on the surface of the substrate, and hardened after heat drying and UV curing to obtain a semi-finished product;
[0061] 2) The AF coating liquid is evenly coated on the semi-finished product, and dried at 140-160° C. for 3-8 minutes to obtain a hardened protective film that can increase the service life of the foldable mobile phone.
[0062] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.
[0063] Example 1
[0064] A hardened protective film capable of prolonging the service life of a foldable mobile phone, and a preparation method thereof comprises the following steps:
[0065] S1. Preparation of nano-silica with surface modified organic siloxane:
[0066] S1-1. At 25°C, a mixture of 5 mL of Triton X-100 (Shanghai Kaiyin Chemical Co., Ltd., other examples and comparative examples have the same source) and n-octanol was mixed with 3 mL of cyclohexane, the mass ratio of Triton X-100 to n-octanol being 1.7:1. Under stirring, 0.9 mL of 25% ammonia water was added dropwise within 20 min to obtain a microemulsion;
[0067] Under stirring, 3 mL of ethyl orthosilicate was added dropwise (the dropping speed was controlled and completed in 30 min), and stirring was continued for 3 h to gradually hydrolyze to generate nano inorganic silica particles. The obtained nano silica was dispersed with anhydrous ethanol to a nano silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method and was 0.9 mmol / g.
[0068] S1-2, take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 0.72 mmol of 3-(isobutyleneoxy)propyltrimethoxysilane (Shanghai MacLean Biochemical Technology Co., Ltd., brand Silane A174, other embodiments and comparative examples have the same source), stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge for multiple times to obtain inorganic particles: nano-silica with surface modified with organic siloxane.
[0069] Wherein, the particle size of nano-silicon dioxide is 10nm.
[0070] The molar ratio between the hydroxyl group (-OH) on the surface of the nano-silica modified with the organic siloxane and the organic siloxane is 8:2.
[0071] According to the mass ratio, 50% of nano-silica with surface modified organic siloxane and 50% of polyurethane acrylic resin (Sartomer Company, brand CN8007NS) were evenly mixed to obtain hardened glue.
[0072] S2. Preparation of AF coating solution:
[0073] S2-1, weigh 50g of perfluoropolyether acyl fluoride (Shanghai MacLean Biochemical Technology Co., Ltd., brand name HFPOOligomer acid fluorides, other examples and comparative examples have the same source) in a reactor, add 100ml of anhydrous methanol, heat to 50°C and react for 2 hours, the whole process is carried out under 1.5 times the atmospheric pressure and nitrogen protection, finally add distilled water for washing until the upper layer is neutral, add dichloromethane and perfluorocyclic ether (Wilbo New Materials Technology (Suzhou) Co., Ltd., other examples and comparative examples have the same source), separate the liquids, filter, and distill under reduced pressure to obtain perfluoropolyether methyl ester;
[0074] Weigh 20 g of the perfluoropolyether methyl ester prepared in step S2-1, then add 20 g of KH550 (Shanghai MacLean Biochemical Technology Co., Ltd., other examples and comparative examples have the same source), react at 60° C. under nitrogen protection for 8 hours, add anhydrous ethanol and perfluorocyclohexane after the reaction, separate the liquids, filter, and perform reduced pressure distillation to obtain a perfluoropolyether aminosiloxane resin, which is then diluted with a perfluoroheptane solvent to a solid content of 10% to obtain an AF coating solution.
[0075] The weight average molecular weight of the fluoropolyether aminosiloxane resin prepared in this embodiment is 10000, and its molecular structure is:
[0076]
[0077] Among them, n=52.
[0078] S3, preparing a hardened protective film;
[0079] S3-1, by slit coating, the hardened glue is evenly coated on the surface of the substrate (PET, U483 of Toray Co., Ltd., Japan, 50 microns thick), and after heat drying (120 degrees, 5 minutes) and UV curing (solid energy of 700mj), hardening forms a hardened coating with a thickness of 5 microns to obtain a semi-finished product;
[0080] S3-2. The AF coating liquid is evenly coated on the semi-finished product through slit coating, and dried at 150°C for 5 minutes to form a fluorine-containing coating with a thickness of 25 nm, thereby obtaining a hardened protective film that can increase the service life of the foldable mobile phone.
[0081] Among them, the dynamic friction coefficient of the fluorine-containing coating surface is 0.01.
[0082] Example 2
[0083] Different from Example 1, the components of the hardened glue in this example are as follows:
[0084] The mass content of the polyurethane acrylic resin is 70%; the mass content of the inorganic particles is 30%.
[0085] Example 3
[0086] Different from Example 1, the thickness of the hardened coating in this example is 3 microns.
[0087] Example 4
[0088] Different from Example 1, the size of the inorganic particles in this example is 20 nm, and the preparation method is as follows:
[0089] S1-1. At 25°C, 5 mL of a mixture of Triton X-100 and n-octanol was mixed with 3 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.9 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0090] Under stirring, 3 mL of ethyl orthosilicate was added dropwise (the dropping speed was controlled and completed in 20 min), and stirring was continued for 3 h to gradually hydrolyze to generate nano inorganic silica particles. The obtained nano silica was dispersed with anhydrous ethanol to a nano silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method and was 0.9 mmol / g.
[0091] S1-2. Take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 0.72 mmol of 3-(isobutyleneoxy)propyltrimethoxysilane, stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge for multiple times to obtain inorganic particles: nano-silica with surface modified organic siloxane.
[0092] Wherein, the particle size of nano-silicon dioxide is 20nm.
[0093] Example 5
[0094] Different from Example 1, the size of the inorganic particles in this example is 30 nm, and the preparation method is as follows:
[0095] S1-1. At 25°C, 5 mL of a mixture of Triton X-100 and n-octanol was mixed with 3 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.9 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0096] Under stirring, 3 mL of ethyl orthosilicate was added dropwise (the dropping speed was controlled and completed in 10 min), and stirring was continued for 3 h to gradually hydrolyze to generate nano inorganic silica particles. The obtained nano silica was dispersed with anhydrous ethanol to a nano silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method and was 0.9 mmol / g.
[0097] S1-2. Take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 0.72 mmol of 3-(isobutyleneoxy)propyltrimethoxysilane, stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge for multiple times to obtain inorganic particles: nano-silica with surface modified organic siloxane.
[0098] Among them, the particle size of nano-silicon dioxide is 30nm.
[0099] Example 6
[0100] Different from Example 1, in this example, the molar ratio between the hydroxyl group (-OH) on the surface of the inorganic particles and the surface-modified organic siloxane is 5:5, and the corresponding preparation method is:
[0101] S1. Preparation of nano-silica with surface modified organic siloxane:
[0102] S1-1. At 25°C, 5 mL of a mixture of Triton X-100 and n-octanol was mixed with 3 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.9 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0103] Under stirring, 3 mL of ethyl orthosilicate was added dropwise, and stirring was continued for 3 h to gradually hydrolyze to generate nano-inorganic silica particles. The obtained nano-silica was dispersed in anhydrous ethanol to a nano-silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method to be 0.9 mmol / g;
[0104] S1-2, take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 1.8 mmol of 3-(isobutyleneoxy)propyltrimethoxysilane, stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge for multiple times to obtain inorganic particles: nano-silica with surface modified organic siloxane.
[0105] Wherein, the particle size of nano-silicon dioxide is 10nm.
[0106] The molar ratio between the hydroxyl group (-OH) on the surface of the nano-silica modified with the organic siloxane and the organic siloxane is 5:5.
[0107] Example 7
[0108] Different from Example 1, the thickness of the fluorine-containing coating in this example is 25 nm.
[0109] Example 8
[0110] Different from Example 1, the thickness of the fluorine-containing coating in this example is 15 nm.
[0111] Example 9
[0112] Different from Example 1, the thickness of the fluorine-containing coating in this example is 7 nm.
[0113] Example 10
[0114] Different from Example 1, the dynamic friction coefficient of the surface of the hardened film protective film in this example is 0.05.
[0115] The weight average molecular weight of the fluoropolyether aminosiloxane resin prepared in this embodiment is 10000, and its molecular structure is:
[0116]
[0117] Among them, n=52.
[0118] In this example, the preparation method of the hardened film is as follows:
[0119] S3-1, by slit coating, the hardened glue is evenly coated on the surface of the substrate (PET, U483 of Toray Co., Ltd., Japan, 50 microns thick), and after heat drying (120 degrees, 5 minutes) and UV curing (solid energy of 700mj), hardening forms a hardened coating with a thickness of 5 microns to obtain a semi-finished product;
[0120] S3-2. The AF coating liquid is evenly coated on the semi-finished product through slit coating, and dried at 150°C for 5 minutes to form a fluorine-containing coating with a thickness of 10 nm, thereby obtaining a hardened protective film that can increase the service life of the foldable mobile phone.
[0121] Among them, the dynamic friction coefficient of the fluorine-containing coating surface is 0.05.
[0122] Embodiment 11
[0123] Different from Example 1, the dynamic friction coefficient of the surface of the hardened film protective film in this example is 0.03.
[0124] The weight average molecular weight of the fluoropolyether aminosiloxane resin prepared in this embodiment is 10000, and its molecular structure is:
[0125]
[0126] Among them, n=52.
[0127] In this example, the preparation method of the hardened film is as follows:
[0128] S3-1, by slit coating, the hardened glue is evenly coated on the surface of the substrate (PET, U483 of Toray Co., Ltd., Japan, 50 microns thick), and after heat drying (120 degrees, 5 minutes) and UV curing (solid energy of 700mj), hardening forms a hardened coating with a thickness of 5 microns to obtain a semi-finished product;
[0129] S3-2. The AF coating liquid is evenly coated on the semi-finished product through slit coating, and dried at 150°C for 5 minutes to form a fluorine-containing coating with a thickness of 20 nm, thereby obtaining a hardened protective film that can increase the service life of the foldable mobile phone.
[0130] Among them, the dynamic friction coefficient of the fluorine-containing coating surface is 0.03.
[0131] Example 12
[0132] Different from Example 1, the substrate in this example is Toray XF7LA7 with a thickness of 65 microns.
[0133] Embodiment 13
[0134] Different from Example 1, the substrate in this example is Toray U483 with a thickness of 75 microns.
[0135] Embodiment 14
[0136] Different from Example 1, the substrate in this example is Toyobo SRF with a thickness of 80 microns.
[0137] Comparative Example 1
[0138] Different from Example 1, the method for preparing the hardened protective film in this example is:
[0139] Through slit coating, the hardened glue (Japanese Arakawa Chemical, brand CH410) is evenly coated on the PET substrate (U483, 50 microns thick) of Japan Toray Corporation. After heat drying (120 degrees, 5 minutes) and UV curing (solid energy of 700mj), a hardened film with a thickness of 5 microns is formed, and a hardened protective film is obtained.
[0140] Comparative Example 2
[0141] Different from Example 1, this example uses KY-1203 produced by Shin-Etsu Chemical of Japan to replace the perfluoropolyether aminosiloxane resin in Example 1.
[0142] Comparative Example 3
[0143] Different from Example 1, the mass content of inorganic particles in the hardened glue in this example is 10%.
[0144] Comparative Example 4
[0145] Different from Example 1, the mass content of inorganic particles in the hardened glue in this example is 70%.
[0146] Comparative Example 5
[0147] Different from Example 1, the size of the inorganic particles in this example is 5 nm, and the preparation method is as follows:
[0148] S1. Preparation of nano-silica with surface modified organic siloxane:
[0149] S1-1. At 25°C, 5 mL of a mixture of Triton X-100 and n-octanol was mixed with 3 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.9 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0150] Under stirring, 3 mL of ethyl orthosilicate was added dropwise (the dropping speed was controlled and completed in 240 min), and stirring was continued for 3 h to gradually hydrolyze to generate nano inorganic silica particles. The obtained nano silica was dispersed with anhydrous ethanol to a nano silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method and was 0.9 mmol / g.
[0151] S1-2. Take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 0.72 mmol of 3-(isobutyleneoxy)propyltrimethoxysilane, stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge for multiple times to obtain inorganic particles: nano-silica with surface modified organic siloxane.
[0152] Among them, the particle size of nano-silicon dioxide is 5nm.
[0153] The molar ratio between the hydroxyl group (-OH) on the surface of the nano-silica modified with the organic siloxane and the organic siloxane is 8:2.
[0154] Comparative Example 6
[0155] Different from Example 1, the size of the inorganic particles in this example is 50 nm, and the preparation method is as follows:
[0156] S1. Preparation of nano-silica with surface modified organic siloxane:
[0157] S1-1. At 25°C, 5 mL of a mixture of Triton X-100 and n-octanol was mixed with 3 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.9 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0158] Under stirring, 3 mL of ethyl orthosilicate was added dropwise (the dropping speed was controlled and completed in 2 min), and stirring was continued for 3 h to gradually hydrolyze to generate nano inorganic silica particles. The obtained nano silica was dispersed with anhydrous ethanol to a nano silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method and was 0.9 mmol / g.
[0159] S1-2. Take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 0.72 mmol of 3-(isobutyleneoxy)propyltrimethoxysilane, stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge for multiple times to obtain inorganic particles: nano-silica with surface modified organic siloxane.
[0160] Wherein, the particle size of nano-silicon dioxide is 50nm.
[0161] The molar ratio between the hydroxyl group (-OH) on the surface of the nano-silica modified with the organic siloxane and the organic siloxane is 8:2.
[0162] Comparative Example 7
[0163] Different from Example 1, the inorganic particles in this example are zirconium oxide with surface modified with organosiloxane. The preparation method is the same as step S1-2 in Example 1, except that zirconium oxide with a particle size of 10 nm is used instead of the nano-silicon dioxide dispersion in step S1-2 of Example 1.
[0164] Comparative Example 8
[0165] Different from Example 1, in this example, the amount of 3-(methacryloyloxy)propyltrimethoxysilane added in step S1-2 is adjusted so that the molar ratio between the hydroxyl group (-OH) on the surface of the inorganic particles and the organic siloxane is 9:1.
[0166] Comparative Example 9
[0167] Different from Example 1, in this example, the amount of 3-(methacryloyloxy)propyltrimethoxysilane added in step S1-2 is adjusted so that the molar ratio between the hydroxyl group (-OH) on the surface of the inorganic particles and the organic siloxane is 2:8.
[0168] Comparative Example 10
[0169] Different from Example 1, the steps for preparing the nano-silica with surface modified with organosiloxane in this example are as follows:
[0170] S1-1. At 25°C, 5 mL of a mixture of Triton X-100 and n-octanol was mixed with 3 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:1. Under stirring, 0.9 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion.
[0171] Under stirring, 3 mL of ethyl orthosilicate was added dropwise, and stirring was continued for 3 h to gradually hydrolyze to generate nano-inorganic silica particles. The obtained nano-silica was dispersed in anhydrous ethanol to a nano-silica dispersion with a solid content of 20%. The hydroxyl content on the surface of the silica was characterized by an acid-base titration method to be 0.9 mmol / g;
[0172] S1-2. Take 20 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 1.8 mmol of trimethoxy (3-methoxypropyl) silane, stir and react at 50°C for 10 hours, centrifuge at 10000 rpm for 1 hour, and after solid precipitation, wash and centrifuge several times to obtain inorganic particles: nano-silica with surface modified organic siloxane.
[0173] Comparative Example 11
[0174] Different from Example 1, the thickness of the fluorine-containing layer in this example is 5 nm.
[0175] Comparative Example 12
[0176] Different from Example 1, the thickness of the fluorine-containing layer in this example is 30 nm.
[0177] Comparative Example 13
[0178] Different from Example 1, the dynamic friction coefficient in this example is 0.07.
[0179] The weight average molecular weight of the fluoropolyether aminosiloxane resin prepared in this example is 5000, and its molecular structure is:
[0180]
[0181] Among them, n=24.
[0182] S3, preparing a hardened protective film;
[0183] S3-1, by slit coating, the hardened glue is evenly coated on the surface of the substrate (PET, U483 of Toray Co., Ltd., Japan, 50 microns thick), and after heat drying (120 degrees, 5 minutes) and UV curing (solid energy of 700mj), hardening forms a hardened coating with a thickness of 5 microns to obtain a semi-finished product;
[0184] S3-2. The AF coating liquid is evenly coated on the semi-finished product through slit coating, and dried at 150°C for 5 minutes to form a fluorine-containing coating with a thickness of 5 nm, thereby obtaining a hardened protective film that can increase the service life of the foldable mobile phone.
[0185] Among them, the dynamic friction coefficient of the fluorine-containing coating surface is 0.07.
[0186] Comparative Example 14
[0187] Different from Example 1, in step S3-2 of this example, the thermal drying and curing conditions of the AF coating liquid are: 100°C, 3 min.
[0188] The performance tests of the protective films prepared in the examples and comparative examples are as follows:
[0189] (1) Steel wool wear test method:
[0190] Grinding head 2cm*2cm, load 1kg, steel wool, brand Bonstar, 0000#, test speed 40 times / minute, with a stroke of about 40mm.
[0191] (2) Test method for eraser wear resistance:
[0192] Use a special rubber (minoan) to apply a load of 1 kg at a speed of 40 times / minute with a stroke of about 40 mm.
[0193] The test results are shown in Table 1 below:
[0194] Table 1
[0195]
[0196]
[0197] According to the test results in Table 1, it can be explained that:
[0198] The thickness of the hardened coating is designed to be 3-5 microns. If the thickness is less than 3 microns, the hardened coating's ability to support wear resistance will decrease, and the wear resistance of the finished steel wool and eraser will decrease, ultimately causing damage to the hardened coating in the wear test or a decrease in the bending test after wear. If the thickness of the hardened coating exceeds 5 microns, although it can increase the ability to resist surface damage due to wear, the bending stress of the hardened coating is large when bending, and it is prone to bending cracking and failure.
[0199] The inorganic particle content in the formula of the hardening coating is 30% or 50%, and the comprehensive performance is the best; the size of the inorganic particles is selected to be 10nm, 20nm, and 30nm. When it is lower than 10nm, the inorganic particles are easy to aggregate, and the mass production yield is low, which is not conducive to industrial mass production. When the particle size exceeds 30nm, the surface roughness of the hardening coating is large, which increases the surface resistance during wear resistance, increases the wear on the surface of the hardened layer during wear resistance, and reduces the bending life.
[0200] The thickness of the fluorine-containing coating is 7-25nm. When it is lower than 7nm, the wear resistance is reduced. When it is higher than 25nm, the appearance is foggy and oily. The dynamic friction coefficient of the surface of the hardened protective film is ≤0.05, and the surface is very smooth, which helps to improve the wear resistance. After testing, the optimal curing conditions for the thermal drying of the fluorine-containing coating liquid are a temperature of 150 degrees and a time of 5 minutes. If the temperature is low and the drying time is short (Comparative Example 14), it is not conducive to the curing reaction of the fluororesin.
[0201] The technical solution of the present invention can improve the ability of the surface of the hardened protective film to resist external wear, thereby increasing the bending resistance life. Moreover, due to the relatively high surface fluorine content, the dynamic friction coefficient is reduced, thereby improving the smoothness, anti-fouling performance and anti-fingerprint ability of consumers when using the touch screen.
[0202] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.
Claims
1. A hardened protective film capable of prolonging the service life of a foldable mobile phone, characterized in that: It includes a substrate, a hardening coating and a fluorine-containing layer which are stacked in sequence; Wherein, the hardened coating is obtained by coating hardened glue and then curing, and the fluorine-containing layer is obtained by coating AF coating liquid and then curing; The hardened glue is a mixture of polyurethane acrylic resin and inorganic particles, and the inorganic particles contain hydroxyl groups and organic siloxane introduced by surface modification; The AF coating liquid is a perfluoropolyether siloxane resin solution.
2. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 1, characterized in that: The molar ratio of the hydroxyl group on the surface of the inorganic particles to the organic siloxane is 8:2 to 5:
5.
3. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 1, characterized in that: The mass percentage of inorganic particles in the hardened glue is 30% to 50%; The inorganic particles are nano-silicon dioxide with a particle size of 10 to 30 nm and surface-modified with organic siloxane.
4. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 3, characterized in that: The organosiloxane is 3-(methacryloyloxy)propyltrimethoxysilane.
5. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 4, characterized in that: The surface-modified nano-silica with organic siloxane is prepared by the following method: S1-1. At 25°C, 2.5-10 mL of a mixture of Triton X-100 and n-octanol was mixed with 1.5-6 mL of cyclohexane, wherein the mass ratio of Triton X-100 to n-octanol was 1.7:
1. Under stirring, 0.45-1.8 mL of 25% aqueous ammonia was added dropwise over 20 min to obtain a microemulsion. Under stirring, 1.5-6 mL of ethyl orthosilicate is added dropwise, stirring is continued for 1.5-6 hours, centrifuged and filtered, and the obtained nano-silicon dioxide is dispersed with anhydrous ethanol to a nano-silicon dioxide dispersion with a solid content of 10-30%. The hydroxyl content on the surface of the obtained nano-silicon dioxide is measured. S1-2, take 10-40 grams of the nano-silica dispersion obtained in step S1-1, add it to 16 grams of deionized water, add 3-(isomethacryloyloxy)propyltrimethoxysilane, control the molar ratio of hydroxyl groups on the surface of the nano-silica to 3-(isomethacryloyloxy)propyltrimethoxysilane to be 8:2-5:5, stir the reaction at 50°C for 5-20 hours, centrifuge at 5000-20000 rpm for 0.5-2 hours, and after solid precipitation, wash and centrifuge for multiple times to obtain nano-silica with surface modified organic siloxane.
6. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 1, characterized in that: The weight average molecular weight of the perfluoropolyether siloxane resin is 5000-10000, and the molecular structure is shown in Formula 1 below: The value range of n is 24-52.
7. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 6, characterized in that: The solid content of the AF coating liquid is 5-20%.
8. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 7, characterized in that: The AF coating solution is prepared by the following method: S2-1, weigh 50g of perfluoropolyether acyl fluoride into a reaction kettle, add 100ml of anhydrous methanol, heat to 50°C and react for 2 hours. The whole process is carried out under 1.5 times the atmospheric pressure and nitrogen protection. Finally, add distilled water for washing until the upper layer is neutral, add dichloromethane and perfluorocyclic ether, separate the liquids, filter, and distill under reduced pressure to obtain perfluoropolyether methyl ester; Weigh 20 g of the perfluoropolyether methyl ester prepared in step S2-1, then add 20 g of KH550, react at 60° C. under nitrogen protection for 8 hours, add anhydrous ethanol and perfluorocyclohexane after the reaction, separate the liquids, filter, and perform reduced pressure distillation to obtain a perfluoropolyether aminosiloxane resin, which is then diluted with a perfluoroheptane solvent to a solid content of 5-20% to obtain the AF coating solution.
9. The hardened protective film capable of prolonging the service life of a foldable mobile phone according to claim 1, characterized in that: in, The thickness of the hardened coating is 3-5 μm; the thickness of the fluorine-containing coating is 7-25 nm, and the dynamic friction coefficient of the surface of the fluorine-containing coating is ≤0.
05.
10. A method for preparing a hardened protective film capable of prolonging the service life of a foldable mobile phone as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: 1) The hardened glue is evenly coated on the surface of the substrate, and hardened after heat drying and UV curing to obtain a semi-finished product; 2) The AF coating liquid is evenly coated on the semi-finished product, and dried at 140-160° C. for 3-8 minutes to obtain the hardened protective film capable of prolonging the service life of the foldable mobile phone.