Hydrophobic foam capable of adsorbing electrolyte and resisting electrolyte corrosion as well as preparation method and application of hydrophobic foam

By introducing carboxylated modified end hydroxy polybutadiene and polyether polyol into polyurethane foam, the porosity and hydrophobic properties are improved, and the problems of hydrophilicity and electrolyte corrosion resistance of polyurethane foam are solved, achieving high efficiency The adsorption electrolyte and waterproof and moisture-resistant effect are suitable for battery protection.

CN118930959APending Publication Date: 2024-11-12HUBEI XIANGYUAN NEW MATERIAL TECH INC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410996690.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing polyurethane foam has strong hydrophilicity, poor waterproof and moisture resistance, and is not resistant to electrolyte corrosion, so it cannot effectively adsorb and deal with the leakage of battery electrolyte.

Method used

Develop a hydrophobic polyurethane foam that improves the porosity, cell size and the size of the foam by introducing carboxylated modified end hydroxy polybutadiene and polyether polyols into the foam and using specific formulations and processes. Hydrophobic properties make it resistant to electrolyte corrosion and effectively adsorb the electrolyte.

Benefits of technology

It achieves high saturation adsorption electrolyte ratio, low water absorption rate and good electrolyte corrosion resistance, extends the cycle life of the battery and prevents the battery from expanding, and is suitable for filling materials between the battery bare battery cell and the shell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930959A_ABST
    Figure CN118930959A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of polyurethane foam materials, and particularly relates to hydrophobic foam capable of adsorbing electrolyte and resisting electrolyte corrosion and a preparation method and application of the hydrophobic foam. The hydrophobic foam provided by the invention is relatively high in porosity, relatively large in cell size and high in electrolyte absorption capacity, and can prevent the electrolyte from leaking to pollute the surrounding environment and damage equipment. Meanwhile, the foam is excellent in water repellency and low in water absorption rate, and can play a role in water resistance and moisture resistance when being applied between the naked battery cell and the cylindrical shell of the battery. Besides, the foam also has certain strength and toughness, the strength loss is small after the foam is soaked in electrolyte, the foam is resistant to electrolyte corrosion, and the internal stress of the battery can be released to a certain extent by extruding the foam, so that the expansion of the battery can be effectively buffered and weakened, and the cycle life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of polyurethane foam materials, and more specifically, relates to a hydrophobic foam capable of absorbing electrolyte and resistant to electrolyte corrosion, and a preparation method and application thereof. Background Art

[0002] The battery cell is the energy source of electric vehicles. When the battery cell is working, it will generate a certain amount of heat. At different temperatures, it will expand and contract to a certain extent. The battery cell will swell to a certain extent. Long-term contact friction between the battery cells may cause the battery cell to be damaged, the electrolyte leakage may cause circuit corrosion, battery failure and even loss of control. Electrolyte leakage will greatly reduce the battery life and cause safety hazards. Applying foam to the outside of the battery cell can absorb the electrolyte, thereby avoiding environmental and equipment pollution, fire and explosion accidents caused by electrolyte leakage.

[0003] In order to protect the battery cells, polymer foam is widely used in the soft pack of the battery pack, between modules, and on the top and bottom of the whole battery pack. During the packaging process of electric vehicle batteries, polyurethane foam is often filled in the outer shell to protect the battery from vibration and impact, while forming a sealed environment to protect the battery from moisture, corrosive agents and solvents. However, the existing polyurethane foam itself is highly hydrophilic and has defects in waterproof and moisture-resistant applications. In addition, the inherent material properties of polyurethane foam make it not resistant to electrolyte corrosion, and its application in the power battery assembly of new energy vehicles is not effective in dealing with battery electrolyte leakage.

[0004] Therefore, it is necessary to develop a polyurethane foam that can absorb electrolyte and resist electrolyte corrosion, buffer and reduce battery expansion, has strong hydrophobicity, and has waterproof and moisture-resistant properties. Summary of the invention

[0005] In view of the defects of the prior art, the purpose of the present application is to provide a hydrophobic foam that can absorb electrolyte and is resistant to electrolyte corrosion, wherein the porosity of the hydrophobic foam is 60% to 85%, the average pore size of the foam is 0.25 mm to 0.66 mm, the saturated electrolyte adsorption rate is 8.91 g / g to 17.41 g / g, the water absorption rate is 10.27% to 15.80%, and the contact angle between the foam and water is 142.10° to 160.47°;

[0006] The compressive strength of the hydrophobic foam under 25% compression deformation is 52KPa to 75KPa, and the compressive strength attenuation rate after being immersed in the electrolyte for 72 hours is 3.36% to 8.61%.

[0007] Preferably, the hydrophobic foam comprises, by weight, 92 to 95 parts of polyol, 0.3 to 0.5 parts of foaming agent, 2 to 5 parts of cross-linking agent, 0.04 to 0.08 parts of catalyst, 1 to 2 parts of surfactant, 1 to 2 parts of color paste and 27 to 45 parts of isocyanate;

[0008] The polyol comprises carboxylated modified hydroxyl-terminated polybutadiene and polyether polyol, and the mass ratio of the carboxylated modified hydroxyl-terminated polybutadiene to the polyether polyol is 1:(2.5-5).

[0009] Preferably, the polyether polyol is selected from polyether polyol A having a hydroxyl value of 110 mg KOH / g to 450 mg KOH / g and polyether polyol B having a hydroxyl value of 25 mg KOH / g to 56 mg KOH / g.

[0010] More preferably, the polyether polyol A is selected from one or more of NJ-305, PTMG, DL-1000D, DL-400, TMN-450, VORANOL T5001 and VORANOL CP450.

[0011] More preferably, the polyether polyol B is selected from one or more of EP-3600, DL-2000D, POP36 / 38, ZR-001, EP-330N, VORANOL4000LM and VORAPELD3201.

[0012] Preferably, the carboxylated modified hydroxy-terminated polybutadiene can enhance the water repellency, compression strength and electrolyte corrosion resistance of the hydrophobic foam when used in the foam.

[0013] Preferably, the foaming agent is water.

[0014] Preferably, the cross-linking agent is at least one selected from glycerol, triethanolamine, 1,4-butanediol, ethylene glycol, 1,6-hexanediol, primary hydroxytetraol and bis-2-(hydroxypropyl)aniline.

[0015] Preferably, the catalyst is selected from at least one of an amine catalyst and an organic metal catalyst.

[0016] Further preferably, the above-mentioned amine catalyst is one or more of triethylenediamine, bis(dimethylamino)propylamine isopropyl alcohol, trimethylethanolamine, pentamethyldipropylenetriamine, dimethylethanolamine and trimethylhydroxyethylethylenediamine.

[0017] More preferably, the above-mentioned organometallic catalyst is selected from one or more of organotin compounds, organobismuth compounds and organozinc compounds.

[0018] Preferably, the above surfactant is silicone.

[0019] Preferably, the isocyanate is selected from modified diisocyanates having an isocyanate content of 30 wt % to 50 wt %.

[0020] More preferably, the modified diisocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate and isophorone diisocyanate.

[0021] The present application also provides a method for preparing the above-mentioned hydrophobic foam, comprising the following steps:

[0022] S1, mixing the polyol, the blowing agent, the cross-linking agent, the catalyst, the surfactant and the color paste according to the ratio to obtain a mixed material A;

[0023] S2, mixing the mixed material A and the isocyanate according to a ratio, and then applying them on the surface of the substrate, performing low-temperature aging and high-temperature aging to obtain a polyurethane foam;

[0024] S3, splitting the polyurethane foam to remove the epidermis to obtain skinless polyurethane foam;

[0025] S4. Spraying polydimethylsiloxane on the surface of the skinless polyurethane foam to obtain a hydrophobic foam.

[0026] Preferably, in step S1, the carboxylated modified hydroxy-terminated polybutadiene is obtained by graft polymerization of hydroxy-terminated polybutadiene and mercaptosuccinic acid.

[0027] Preferably, in step S2, the low-temperature aging temperature is 50°C to 65°C, and the time is 5min to 8min.

[0028] Preferably, in step S2, the high temperature aging temperature is 80°C to 100°C, and the time is 10 min to 20 min.

[0029] The present application also provides a foam for filling the gap between a bare battery cell and a shell, which comprises the above-mentioned hydrophobic foam.

[0030] In general, the above technical solutions conceived by this application have the following beneficial effects compared with the prior art:

[0031] (1) The hydrophobic foam provided in the present application, which can absorb electrolyte and resist electrolyte corrosion, has a high porosity, a large pore size, and a strong ability to absorb electrolyte, and can prevent leakage of electrolyte from polluting the surrounding environment and damaging the equipment. At the same time, the foam has excellent water repellency and low water absorption. When applied between the bare battery cell and the cylindrical shell of the battery, it can play a role in waterproofing and moisture resistance. In addition, the foam also has certain strength and toughness, and the strength loss is small after soaking in electrolyte, and it is resistant to electrolyte corrosion. The internal stress of the battery can be released to a certain extent by squeezing the foam, thereby effectively buffering and reducing battery expansion, and extending the battery cycle life. Specifically, the porosity of the hydrophobic foam is 60% to 85%, the average pore size is 0.25 mm to 0.66 mm, the saturated electrolyte adsorption ratio is 8.91 g / g to 17.41 g / g, the water absorption rate is 10.27% to 15.80%, the contact angle between the foam and water is 142.10° to 160.47°, the compressive strength under 25% compression deformation is 52 KPa to 75 KPa, and the compressive strength attenuation rate after immersion in the electrolyte for 72 hours is 3.36% to 8.61%.

[0032] (2) In the hydrophobic foam formula provided in the present application, carboxylated modified terminal hydroxyl polybutadiene is added as a raw material for preparing the foam, and the mass ratio of carboxylated modified terminal hydroxyl polybutadiene and polyether polyol is adjusted, and then compounded with components such as a blowing agent, a catalyst, a surfactant, a color paste and a modified isocyanate. Through the synergistic effect between the components, the foam can take into account the performance of high saturated electrolyte adsorption rate, strong water repellency, and resistance to electrolyte corrosion, and the strength loss after immersion in the electrolyte is small, which can effectively play a role in buffering and reducing battery expansion, and is suitable for use as a foam to fill the gap between the bare battery cell and the shell.

[0033] (3) The preparation method of the hydrophobic foam provided in the present application effectively solves the problems of poor electrolyte absorption effect, electrolyte corrosion resistance, and poor hydrophobicity of existing foams through formula and process adjustment. At the same time, the preparation method provided in the present application has the advantages of simple operation process and low processing difficulty, and can be mass-produced.

[0034] (4) In the preferred embodiment, the present application improves the porosity and pore size of the foam, the ability of the foam to absorb electrolyte, the resistance to electrolyte corrosion and the hydrophobicity of the foam, and at the same time ensures that the foam still has a certain compressive strength after being soaked in electrolyte, thereby having the effect of buffering and reducing battery expansion. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1is the reaction equation for preparing carboxylated modified hydroxy-terminated polybutadiene in the present application;

[0036] Figure 2 It is a nuclear magnetic resonance structure characterization test diagram of the carboxylated modified hydroxyl-terminated polybutadiene in this application;

[0037] Figure 3 This is a nuclear magnetic resonance structure characterization test diagram of the hydroxy-terminated polybutadiene in this application;

[0038] Figure 4 It is a preparation flow chart of the hydrophobic foam provided in this application;

[0039] Figure 5 This is the state of the foam HSN1 prepared in comparative example 1 of the present application after being immersed in the electrolyte for 72 hours. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application specification are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0042] Unless otherwise indicated, all numerical values ​​used in the specification and claims to express the amount of ingredients, reaction conditions, etc. are understood to be modified by the term "about". Therefore, unless otherwise indicated, the numerical parameters set forth herein are approximate values ​​that can vary depending on the desired performance required. Numerical ranges expressed as endpoints include all numbers within the range and any range within the range, for example, 1 to 5 include 1, 1.2, 2.8, 3.5, 4.6 and 5, etc.

[0043] The lithium battery electrolyte used on the market is composed of solvents, solutes and additives, of which the solvent accounts for more than 80% of the total mass of the electrolyte. The electrolyte has a high dielectric constant, extremely high polarity and good dissolving ability. As a polar substance, polyurethane foam can adsorb electrolyte according to the principle of similar polarity dissolving. However, its adsorption capacity is limited by the properties of the foam components, the thickness of the epidermis, the porosity and the size of the pores determined by the formula, which makes it poor in adsorbing electrolyte and not resistant to electrolyte corrosion. A large number of strongly polar groups, hydroxyl groups, are introduced into polyurethane foam during the preparation process, and the main chain structure contains a large number of easily hydrolyzed polar groups such as carbamate and urea, which can show strong polarity when forming hydrogen bonds. Water is a strong polar solvent. According to the principle of similar dissolving, polyurethane foam itself has strong hydrophilicity and poor waterproof and moisture resistance. In order to solve the problems that the existing polyurethane foam itself has poor waterproof effect and is not resistant to electrolyte corrosion, a high adsorption rate of the foam to the electrolyte is achieved, and the foam is resistant to electrolyte corrosion. The foam can still maintain a certain strength when immersed in the electrolyte to play a buffering and weakening expansion role. At the same time, the water absorption rate of the foam is low, and the foam surface has super hydrophobicity, which can play a waterproof and moisture-resistant effect. Based on this, the present application provides a hydrophobic foam that can absorb electrolyte and is resistant to electrolyte corrosion, wherein the porosity is 60% to 85%, the average pore size of the foam is 0.25 mm to 0.66 mm, the saturated electrolyte adsorption ratio is 8.91 g / g to 17.41 g / g, the water absorption rate is 10.27% to 15.80%, and the contact angle between the foam and water is 142.10° to 160.47°; the compressive strength of the hydrophobic foam under 25% compression deformation is 52 KPa to 75 KPa, and the compressive strength attenuation rate after immersion in the electrolyte for 72 hours is 3.36% to 8.61%.

[0044] In some embodiments, the hydrophobic foam comprises, by weight, 92 to 95 parts of polyol, 0.3 to 0.5 parts of foaming agent, 2 to 5 parts of cross-linking agent, 0.04 to 0.08 parts of catalyst, 1 to 2 parts of surfactant, 1 to 2 parts of color paste and 27 to 45 parts of isocyanate; wherein the polyol comprises carboxylated modified terminal hydroxyl polybutadiene and polyether polyol.

[0045] In some embodiments, the carboxylated modified hydroxy-terminated polybutadiene can enhance the water repellency, compression strength and electrolyte corrosion resistance of the hydrophobic foam when used in the foam.

[0046] Through experiments, the present application discovered that by selecting carboxylated-modified terminal hydroxyl polybutadiene as the raw material for preparing hydrophobic polyurethane foam, the water repellency of the foam can be improved by embedding polyolefin chain segments in the foam structure. At the same time, the introduced carboxyl group can undergo a series reaction of acid-base reaction and nucleophilic addition with the isocyanate group to construct a new carbon-nitrogen bond, generate urea and isourea products, and improve the compressive strength and toughness of the polyurethane foam, and improve the foam's resistance to electrolyte corrosion.

[0047] In some embodiments, the molecular weight of the carboxylated modified hydroxyl-terminated polybutadiene is 2444-7386, and the molecular formula is as follows:

[0048]

[0049] Among them, the ratio of b:(a+b) is (32.9~83.2):100.

[0050] It is to be understood that the present application does not limit the source of the above-mentioned carboxylated modified hydroxy-terminated polybutadiene, which can be purchased from the market or prepared by methods known to those skilled in the art.

[0051] In some embodiments, the polyether polyol includes a polyether polyol A having a hydroxyl value of 112 mg KOH / g to 450 mg KOH / g and a polyether polyol B having a hydroxyl value of 25 mg KOH / g to 56 mg KOH / g. The inventors of the present application found in experiments that when the carboxylated modified hydroxyl-terminated polybutadiene is compounded with a low hydroxyl polyether polyol and a high hydroxyl polyether polyol, the strength of the prepared foam is too low or the toughness is insufficient, and it cannot play a role in buffering and reducing battery expansion. By using a high hydroxyl polyether polyol and a low hydroxyl polyether polyol as the main material of the foam, the polyolefin structure in the carboxylated modified hydroxyl-terminated polybutadiene can be uniformly blended with the polyether phase in the polyether polyol, and the prepared foam has a certain strength and toughness. When the foam is applied between the bare battery cell and the cylindrical shell, it can play a role in buffering and reducing battery expansion.

[0052] In some embodiments, the polyether polyol A is selected from one or more of NJ-305, PTMG, DL-1000D, DL-400, TMN-450, VORANOL T5001 and VORANOL CP450.

[0053] In some embodiments, the polyether polyol B is selected from one or more of EP-3600, DL-2000D, POP36 / 38, ZR-001, EP-330N, VORANOL4000LM and VORAPELD3201.

[0054] In some embodiments, the mass ratio of the polyether polyol A to the polyether polyol B is 1:(1.5-5.5), preferably 1:(1.6-5.3).

[0055] In some embodiments, the mass ratio of the above-mentioned carboxylated modified hydroxyl-terminated polybutadiene and the above-mentioned polyether polyol is 1:(2.5-5). Polyurethane is composed of a soft segment and a hard segment, and there is a microphase separation structure between the soft and hard segments; the polyolefin structure in the molecular chain of carboxylated modified hydroxyl-terminated polybutadiene (HTPB) is a flexible structure, and there is a large difference in the flexibility of polyether polyol and carboxylated modified HTPB, and the copolymerization is poor. The inventors of this application found through experiments that when the amount of carboxylated modified HTPB in the foam formula is low, the soft segment region (the polyolefin structure in the carboxylated modified HTPB and the polyether phase region in the polyether polyol) can be blended relatively uniformly, thereby improving the compression strength of the foam, but the addition amount of carboxylated modified HTPB is too low to improve the ability of the foam to resist electrolyte corrosion; when the amount of carboxylated modified HTPB in the foam formula is high, the structure of the foam is prone to unevenness, which increases the defects in the soft segment phase region, thereby reducing the compression strength of the foam and failing to play a role in slowing down battery expansion.

[0056] In some embodiments, the foaming agent is water.

[0057] It should be understood that the present application does not limit the specific types of cross-linking agents, and any cross-linking agent reported in the prior art may be used. In some embodiments, the cross-linking agent may be, but is not limited to, glycerol, triethanolamine, 1,4-butanediol, ethylene glycol, 1,6-hexanediol, primary hydroxy tetraol, bis-2-(hydroxypropyl) aniline, and other diols, polyols, alcoholamines, and diamines that can be used as cross-linking agents.

[0058] In some embodiments, the catalyst is selected from at least one of an amine catalyst and an organic metal catalyst.

[0059] In a preferred embodiment, the amine catalyst includes but is not limited to triethylenediamine, bis(dimethylamino)propylamine isopropyl alcohol, trimethylethanolamine, pentamethyldipropylenetriamine, dimethylethanolamine and trimethylhydroxyethylethylenediamine.

[0060] In a preferred embodiment, the above-mentioned organic metal catalyst is selected from at least one of an organic tin compound, an organic bismuth compound or an organic zinc compound, such as but not limited to stannous octoate, dibutyltin dilaurate, dibutyltin diacetate, di(dodecylsulfide)dibutyltin, zinc octoate, and potassium acetate.

[0061] In the present application, the mass fraction of the catalyst in the above-mentioned hydrophobic foam is 0.04 to 0.08 parts, the purpose of which is to prolong the time required for the foam maturation and molding, and control the temperature and time of the foam maturation and molding process in two stages, namely low-temperature maturation and high-temperature maturation, so that the foam has the characteristics of high porosity and large pore size.

[0062] It should be understood that the present application does not limit the specific type of surfactant, and any surfactant reported in the prior art may be used, such as but not limited to silicone.

[0063] In some embodiments, the isocyanate is selected from modified diisocyanate with an isocyanate content of 30% to 50%.

[0064] In a preferred embodiment, the modified diisocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate and isophorone diisocyanate.

[0065] The present application also provides a method for preparing the above-mentioned hydrophobic foam, comprising the following steps:

[0066] S1. Mix the above-mentioned polyol, foaming agent, cross-linking agent, catalyst, surfactant and color paste according to the proportion to prepare mixed material A.

[0067] In some embodiments, the polyols include carboxylated modified hydroxy-terminated polybutadiene and polyether polyols. It is to be understood that the present application does not limit the source of the carboxylated modified hydroxy-terminated polybutadiene, which can be purchased commercially or prepared by methods known to those skilled in the art, for example, by graft polymerization of hydroxy-terminated polybutadiene containing carbon-carbon double bonds and thiocarboxylic acid compounds containing sulfhydryl and carboxyl groups, and under photoinitiation conditions, the carbon-carbon double bonds and sulfhydryl (active groups) are grafted to react, thereby introducing a large number of carboxyl groups to synthesize carboxylated modified hydroxy-terminated polybutadiene.

[0068] In some embodiments, the method for preparing carboxylated modified hydroxy-terminated polybutadiene is as follows: hydroxy-terminated polybutadiene is reacted with mercaptosuccinic acid under ultraviolet light initiation conditions, wherein the carbon-carbon double bonds on the hydroxy-terminated polybutadiene molecular chains are grafted with the thiol groups (active groups) of the mercaptosuccinic acid, so that the carboxyl groups connected to the thiol groups in the mercaptosuccinic acid molecular chains are introduced into the hydroxy-terminated polybutadiene molecular chains, thereby preparing modified hydroxy-terminated polybutadiene with a large number of carboxyl groups, i.e., carboxylated modified hydroxy-terminated polybutadiene (carboxylated modified HTPB).

[0069] In some embodiments of the present application, the reaction equation for preparing carboxylated modified HTPB is as follows: Figure 1 As shown, the preparation method is as follows: terminal hydroxyl polybutadiene, mercaptosuccinic acid, 2-methyl-4-(methylthio)phenyl-1-propanone and methanol are mixed, the mixed solution is irradiated with ultraviolet light under the protection of inert gas for modification reaction to obtain a reaction solution, the reaction solution is spin-dried, the spin-dried product is washed with water using a solvent to remove impurities, and then dried to obtain carboxylated modified terminal hydroxyl polybutadiene.

[0070] In some embodiments, the mass ratio of hydroxy-terminated polybutadiene, mercaptosuccinic acid and 2-methyl-4-(methylthio)phenyl-1-propanone is (0.8-1.2):(4-5):(0.08-0.12).

[0071] In some embodiments, the molecular weight of the hydroxy-terminated polybutadiene is 1500-5000.

[0072] In some embodiments, the concentration of mercaptosuccinic acid in the mixed solution is 0.1 g / mL to 0.17 g / mL.

[0073] In some embodiments, the ultraviolet light irradiation time is 2 hours to 12 hours.

[0074] In a specific embodiment of the present application, the preparation method of the above-mentioned carboxylated modified HTPB is as follows: using terminal hydroxyl polybutadiene and mercaptosuccinic acid as starting materials, 2-methyl-4-(methylthio)phenyl-1-propanone as a photoinitiator, and methanol as a solvent, after mixing the above reagents, nitrogen is filled at room temperature, and the reaction is carried out under ultraviolet light irradiation, and the reaction solution is spin-dried, and the spin-dried product is fully washed with a solvent to remove impurities of methanol and excess mercaptosuccinic acid, and then dried to obtain a carboxylated modified HTPB. The molecular weight of the carboxylated modified terminal hydroxyl polybutadiene prepared in the present application is 2444-7386, and the reaction efficiency of the modification is 32.9%-83.2%, that is, the ratio of b:(a+b) in the molecular formula is (32.9-83.2):100.

[0075] S2. Mix the mixed material A and the isocyanate according to the ratio, apply them on the surface of the substrate, and perform low-temperature aging and high-temperature aging to obtain polyurethane foam.

[0076] The foaming process of polyurethane foam can be divided into three stages: initial, middle and late stages. In the initial stage, the bubbles are just formed, and the polymer melt itself has a certain strength and viscoelasticity, which will form resistance to the growth of bubbles and restrict the growth of bubbles. At this time, the growth rate of the bubbles is slow and the growth degree is also low; in the middle and late stages, as the reaction proceeds, a large amount of gas diffuses to the bubble nucleus, and the bubbles grow rapidly. This stage is the main period of bubble growth. The foaming temperature of traditional polyurethane foam is about 100°C. The foaming temperature will affect the melt viscosity, surface tension and diffusivity of carbon dioxide of the polymer, thereby affecting the pore size and porosity of the foam. The present application controls the foaming process of polyurethane foam into two stages from a process perspective. The first stage is low-temperature aging at a temperature of 50°C to 65°C for 5 minutes to 8 minutes. At this time, the strength and viscoelasticity of the polyurethane are extremely low, the surface tension is small, and the resistance to the growth of bubbles is small, which is conducive to the growth of bubbles, so that the foam has a higher porosity and a larger pore size; the second stage is high-temperature aging at a temperature of 80°C to 100°C for 10 minutes to 20 minutes, which ensures that the reaction is completely cured, so that the foam is fully matured and has a certain strength.

[0077] It is to be understood that the present application does not limit the material type of the above-mentioned substrate, and any type of substrate reported in the prior art can be used. The present application does not limit the method of "applying" in step S2, such as but not limited to coating, brushing, dipping, spraying, roller coating, blade coating, flow coating, pouring, printing, and transfer. In a specific embodiment of the present application, the above-mentioned mixed material A is mixed with the above-mentioned isocyanate, and then coated and formed by a coating machine, and then subjected to a aging treatment.

[0078] S3, splitting the polyurethane foam to remove the epidermis to obtain skinless polyurethane foam.

[0079] The purpose of the above-mentioned splitting treatment and removal of the epidermis in the present application is to expose the pores of the foam, so that the electrolyte can more easily infiltrate the foam, thereby effectively improving the foam's ability to absorb the electrolyte; at the same time, the roughness of the surface of the polyurethane foam after splitting is greatly improved, which is very beneficial for the subsequent spraying of polydimethylsiloxane, thereby improving the water repellency of the foam.

[0080] S4. Spraying polydimethylsiloxane on the surface of the skinless polyurethane foam to obtain a hydrophobic foam.

[0081] According to the surface wettability mechanism, the wettability of the foam surface mainly depends on the surface chemical properties and surface microstructure. This application starts from two aspects. By performing a layer-splitting treatment on the polyurethane foam, a skinless polyurethane foam with a high surface roughness is obtained to increase the contact angle between the foam and water. At the same time, polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam. The surface tension of the siloxane segment in the polydimethylsiloxane is low and has strong hydrophobicity. It can be attached to the rough structure surface of the foam as a low surface energy substance, so that the foam forms a hydrophobic surface. The hydrophobic foam provided by this application is used between the bare battery cell and the cylindrical shell, which can play a role in waterproofing and moisture resistance.

[0082] On the other hand, the present application also provides a foam for filling the gap between a bare battery cell and a shell, which comprises the above-mentioned hydrophobic foam.

[0083] It should be understood that, according to the principle of like dissolves like, the hydrophobic foam prepared in the present application has excellent saturated electrolyte adsorption performance and corrosion resistance for any type of electrolyte. Therefore, the present application has no special restrictions on the type of the above-mentioned electrolyte. Any liquid electrolyte reported in the prior art with EC, DMC, PC, DEC or EC / DMC mixture, PC / DMC mixture, etc. as solvent and LiPF6, LiBF6, etc. as conductive salt solute can be used.

[0084] The above technical solutions are described in detail below in conjunction with specific embodiments. It should be understood that these are merely exemplary and are not intended to limit the present application. Materials identical or similar to the types, models, qualities, properties or functions of the following reagents and instruments can be used to implement the present application. The experimental methods used in the following embodiments and comparative examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following embodiments and comparative examples, unless otherwise specified, can all be obtained from commercial sources.

[0085] The following are examples and comparative examples:

[0086] The specific information of the reagents used in the examples and comparative examples of the present application is as follows:

[0087] The reagents used to prepare carboxylation-modified HTPB are as follows: terminal hydroxyl polybutadiene (99%) was purchased from McLean Biochemical Technology Co., Ltd., with a number average relative molecular weight (VPO) of 2500-2817, a hydroxyl value of 75 mg KOH / g, and a functionality of 3.6; mercaptosuccinic acid (98%) was purchased from Jiuding Chemical; 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone (98%) was purchased from Bid Pharmaceutical Technology Co., Ltd.; methanol (99.5%) was purchased from McLean Biochemical Technology Co., Ltd.; tetrahydrofuran (99%) was purchased from McLean Biochemical Technology Co., Ltd.; petroleum ether (AR) was purchased from Inokai Technology Co., Ltd.

[0088] The reagents used to prepare the hydrophobic foam are as follows: NJ-305 was purchased from Jurong Wuning New Materials Co., Ltd., with the brand name NJ-305, a hydroxyl value of 330 mg KOH / g, a functionality of 3, and a molecular weight of 510; PTMG was purchased from Mitsubishi Chemical Corporation, with the brand name PTMG, a hydroxyl value of 112.5 mg KOH / g, and a molecular weight of 1000; DL-1000D was purchased from Shandong Bluestar Dongda Co., Ltd., with the brand name DL-1000D, a hydroxyl value of 112 mg KOH / g; DL-400 was purchased from Shandong Bluestar Dongda Co., Ltd., with the brand name DL-400, a hydroxyl value of 280 mg KOH / g; TNM-450 was purchased from Sanshi (Tianjin) Chemical Technology Co., Ltd., with the brand name TNM-450, a hydroxyl value of 450 mg KOH / g; VORANOLT5001 was purchased from Dow Chemical Company, with the brand name VORANOLT5001, a hydroxyl value of 275 mg KOH / g, functionality is 3, molecular weight is 600; VORANOLCP450 purchased from Dow Chemical Company, brand VORANOLCP450, hydroxyl value is 383mgKOH / g, molecular weight is 450; EP-3600 purchased from Shandong Bluestar Dongda Co., Ltd., brand EP-3600, hydroxyl value is 28mg KOH / g, functionality is 3, molecular weight is 6000; DL-2000D purchased from Shandong Bluestar Dongda Co., Ltd., brand DL-2000D, hydroxyl value is 56mg KOH / g; POP36 / 38 purchased from Shandong Bluestar Dongda Co., Ltd., brand POP36 / 38, hydroxyl value is 25.5mg KOH / g; ZR-001 purchased from Shandong Bluestar Dongda Co., Ltd., brand ZR-001, hydroxyl value is 26.5mg KOH / g; EP-330N was purchased from Shandong Bluestar Dongda Co., Ltd., with the brand name EP-330N and a hydroxyl value of 34mg KOH / g; VORANOL4000LM was purchased from Dow Chemical Company, with the brand name VORANOL4000LM and a hydroxyl value of 28mg KOH / g, a functionality of 2, and a molecular weight of 4000; VORAPELD3201 was purchased from Dow Chemical Company, with the brand name VORAPELD3201 and a hydroxyl value of 56mg KOH / g, functionality is 2, molecular weight is 2000; triethylenediamine was purchased from Xindian Chemical Materials (Shanghai) Co., Ltd.; bis(dimethylaminopropyl)amine isopropanol was purchased from Hangzhou Keying Chemical, No. KY154918; stannous octoate was purchased from Evonik, Germany; dibutyltin dilaurate was purchased from Xindian Chemical Materials (Shanghai) Co., Ltd.; propylene glycol was purchased from Covestro AG; triethanolamine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; 1,4-butanediol was purchased from Shanghai Yuanye Biotechnology Co., Ltd., No. S24138; silicone was purchased from Dow Chemical Company, brand DC6070; toluene diisocyanate TDI-80 was purchased from Covestro Polymer (China) Co., Ltd., brand Desmodur T80, NCO content 48wt%; diphenylmethane diisocyanate MDI-50 was purchased from BASF AG, brand Lupranate MI, NCO content 33.5wt%; polydimethylsiloxane (PDMS) was purchased from Dow Corning, USA.

[0089] Example 1

[0090] The reaction equation for preparing carboxylated modified HTPB is as follows: Figure 1 As shown, the specific preparation method is as follows:

[0091] Weigh 1.029g of hydroxy-terminated polybutadiene, 4.123g of mercaptosuccinic acid, and 0.104g of 2-methyl-4-(methylthio)phenyl-1-propanone into a two-necked flask, add 30mL of methanol, stir and mix, then fill with nitrogen at room temperature, react under ultraviolet light for 8h, spin dry the obtained solution, then use ethyl acetate to wash thoroughly to remove impurity methanol and excess mercaptosuccinic acid, spin dry to obtain a modified polymer with higher purity. Use tetrahydrofuran and petroleum ether as solvents to dissolve and precipitate the modified polymer, dry the precipitated modified polymer, and use dimethyl sulfoxide as solvent to perform nuclear magnetic resonance structural characterization (1H-NMR) test, and the nuclear magnetic resonance hydrogen spectrum is shown in Figure 2 .

[0092] The peak intensity on the hydrogen spectrum is proportional to the number of hydrogen atoms. The number of structural units can be calculated by the number of double bond hydrogens. Figure 2 ) and raw material hydroxyl-terminated polybutadiene ( Figure 3) can be found in the H NMR spectrum that after 8h of reaction, the peak of double bond hydrogen becomes significantly weaker, that is, the remaining double bond ratio becomes significantly less. Since the ratio of the peak area signal value of the hydroxyl adjacent hydrogen to the double bond hydrogen is fixed, the peak area of ​​the hydroxyl adjacent hydrogen is set to 1. The remaining double bond hydrogen ratio can be obtained by integrating the peak area, and then the relative value of the remaining double bond hydrogen of the product can be compared to calculate the reaction efficiency of the modification. The calculation results are shown in Table 1.

[0093] Table 1 Calculation table of reaction degree integral of H NMR spectrum

[0094] sample Solvent system Hydroxyl ortho hydrogen Double bond hydrogen Double bond reaction ratio Double bond remaining ratio Reaction efficiency HTPB <![CDATA[CD3Cl]]> 1 21.28 0 100% 0 Carboxylated modified HTPB DMSO 1 3.57 83.20% 16.80% 83.2%

[0095] As can be seen from Table 1, the reaction efficiency of the modification method provided by the present application is 83.2%, that is, the ratio of b:(a+b) is 83.2:100, indicating that the modification of the present application is successful and carboxylated modified hydroxy-terminated polybutadiene (carboxylated modified HTPB) can be prepared, and its number average molecular weight is 2246-4546.

[0096] 1) The hydrophobic foam provided in the embodiment of the present application includes, by weight, 23 parts of carboxylated modified HTPB (the ratio of b:(a+b) is 83.2:100), 15 parts of NJ-305, 55 parts of EP-3600, 1.65 parts of silicone, 0.05 parts of stannous octoate, 3 parts of propylene glycol, 0.3 parts of water, 2 parts of color paste and 32 parts of toluene diisocyanate TDI-80.

[0097] 2) The preparation method of polyurethane foam comprises the following steps: Figure 4 ):

[0098] S1. The carboxylated modified HTPB, NJ-305, EP-3600, silicone, stannous octoate, glycerol, water and color paste are uniformly stirred according to a proportion to obtain a mixed material A;

[0099] S2. Mix the mixed material A with toluene diisocyanate TDI-80, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 60°C for 5 minutes, and the second stage is high-temperature aging at a temperature of 95°C for 10 minutes to obtain polyurethane foam.

[0100] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0101] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam PU-1.

[0102] Example 2

[0103] 1) The hydrophobic foam provided in the embodiment of the present application includes, by mass, 26.6 parts of carboxylated modified HTPB (same as in Example 1), 13 parts of NJ-305, 53.4 parts of EP-3600, 1.8 parts of silicone, 0.06 parts of dimethylaminopropylamine isopropanol, 2.8 parts of triethanolamine, 0.34 parts of water, 2 parts of color paste and 45 parts of diphenylmethane diisocyanate MDI-50.

[0104] 2) The preparation method of the hydrophobic foam comprises the following steps:

[0105] S1. Mix carboxylated modified HTPB, NJ-305, EP-3600, silicone, dimethylaminopropylamine isopropyl alcohol, triethanolamine, water and color paste according to the proportion to obtain mixed material A;

[0106] S2. Mix the mixed material A with toluene diisocyanate TDI-80, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 55°C for 6 minutes, and the second stage is high-temperature aging at a temperature of 85°C for 15 minutes to obtain polyurethane foam.

[0107] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0108] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam PU-2.

[0109] Example 3

[0110] 1) The hydrophobic foam provided in the embodiment of the present application includes, by weight, 18.4 parts of carboxylated modified HTPB (same as in Example 1), 16 parts of NJ-305, 57.6 parts of EP-3600, 1.93 parts of silicone, 0.07 parts of dibutyltin dilaurate, 3.6 parts of 1,4-butanediol, 0.4 parts of water, 2 parts of color paste and 27 parts of toluene diisocyanate TDI-80.

[0111] 2) The preparation method of the hydrophobic foam comprises the following steps:

[0112] S1. The carboxylated modified HTPB, NJ-305, EP-3600, silicone, dibutyltin dilaurate, 1,4-butanediol, water and color paste are uniformly mixed according to a proportion to obtain a mixed material A;

[0113] S2. Mix the mixed material A with toluene diisocyanate TDI-80, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 50°C for 8 minutes, and the second stage is high-temperature aging at a temperature of 100°C for 10 minutes to obtain polyurethane foam.

[0114] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0115] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam PU-3.

[0116] Example 4

[0117] 1) The hydrophobic foam provided in the embodiment of the present application includes, by mass, 20.67 parts of carboxylated modified HTPB (same as in Example 1), 18 parts of NJ-305, 54.33 parts of EP-3600, 1.57 parts of silicone, 0.08 parts of dimethylaminopropylamine isopropanol, 3 parts of glycerol, 0.35 parts of water, 2 parts of color paste and 38 parts of diphenylmethane diisocyanate MDI-50.

[0118] 2) The preparation method of the hydrophobic foam comprises the following steps:

[0119] S1. Mix carboxylated modified HTPB, NJ-305, EP-3600, silicone, dimethylaminopropylamine isopropyl alcohol, glycerol, water and color paste according to the proportion to obtain mixed material A;

[0120] S2. Mix the mixed material A with toluene diisocyanate TDI-80, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 65°C for 5 minutes, and the second stage is high-temperature aging at a temperature of 80°C for 15 minutes to obtain polyurethane foam.

[0121] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0122] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam PU-4.

[0123] Example 5

[0124] 1) The hydrophobic foam provided in the embodiment of the present application includes, by weight, 20.49 parts of carboxylated modified HTPB (same as in Example 1), 13 parts of NJ-305, 58.71 parts of EP-3600, 1.73 parts of silicone, 0.03 parts of stannous octoate, 0.03 parts of dibutyltin dilaurate, 4.1 parts of triethanolamine, 0.31 parts of water, 1.6 parts of color paste and 28 parts of toluene diisocyanate TDI-80.

[0125] 2) The preparation method of the hydrophobic foam comprises the following steps:

[0126] S1. The carboxylated modified HTPB, NJ-305, EP-3600, silicone, stannous octoate, dibutyltin dilaurate, triethanolamine, water and color paste are uniformly stirred according to a proportion to obtain a mixed material A;

[0127] S2. Mix the mixed material A with toluene diisocyanate TDI-80, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 55°C for 6 minutes, and the second stage is high-temperature aging at a temperature of 90°C for 15 minutes to obtain polyurethane foam.

[0128] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0129] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam PU-5.

[0130] Example 6

[0131] 1) The hydrophobic foam provided in the embodiment of the present application includes, by mass, 15.55 parts of carboxylated modified HTPB (same as in Example 1), 19 parts of NJ-305, 58.75 parts of EP-3600, 1.55 parts of silicone, 0.04 parts of trimethylethylenediamine, 0.03 parts of dimethylaminopropylamine isopropanol, 2.7 parts of 1,4-butanediol, 0.38 parts of water, 2 parts of color paste and 36 parts of diphenylmethane diisocyanate MDI-50.

[0132] 2) The preparation method of the hydrophobic foam comprises the following steps:

[0133] S1. The carboxylated modified HTPB, NJ-305, EP-3600, silicone, trimethylethylenediamine, bis(dimethylaminopropyl)amine isopropanol, 1,4-butanediol, water and color paste are uniformly mixed according to a proportion to obtain a mixed material A;

[0134] S2. Mix the above mixed material A with diphenylmethane diisocyanate MDI-50, apply coating to form the mixture through a coating machine, and perform aging treatment after coating to make it foamed and formed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 50°C for 7 minutes, and the second stage is high-temperature aging at a temperature of 95°C for 20 minutes to obtain polyurethane foam.

[0135] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0136] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam PU-6.

[0137] Embodiments 7 to 9

[0138] The raw materials of the hydrophobic foams provided in Examples 7 to 9 of the present application and the mass fractions of each raw material are listed in Table 2. Finished foams PU-7, PU-8, and PU-9 were obtained according to the preparation method of Example 1.

[0139] Table 2 Raw materials of hydrophobic foam provided in Examples 7 to 9 and the mass fraction of each raw material

[0140]

[0141] Comparative Example 1

[0142] The foam provided in this comparative example includes, by weight, 22 parts of NJ-305, 71 parts of EP-3600, 1.65 parts of silicone, 0.05 parts of stannous octoate, 3 parts of propylene glycol, 0.3 parts of water, 2 parts of color paste and 48 parts of toluene diisocyanate TDI-80.

[0143] The preparation method of the foam is the same as that of Example 1, and a finished foam HSN1 is obtained.

[0144] Comparative Example 2

[0145] The foam provided in this comparative example includes, by weight, 31 parts of carboxylated modified HTPB (same as Example 1), 17 parts of NJ-305, 45 parts of EP-3600, 1.65 parts of silicone, 0.05 parts of stannous octoate, 3 parts of propylene glycol, 0.3 parts of water, 2 parts of color paste and 24 parts of toluene diisocyanate TDI-80.

[0146] The preparation method of the foam is the same as that of Example 1, and a finished foam HSN2 is obtained.

[0147] Comparative Example 3

[0148] The foam provided in this comparative example includes, by weight, 14.3 parts of carboxylated modified HTPB (same as Example 1), 17 parts of NJ-305, 61.7 parts of EP-3600, 1.65 parts of silicone, 0.05 parts of stannous octoate, 3 parts of propylene glycol, 0.3 parts of water, 2 parts of color paste and 44 parts of toluene diisocyanate TDI-80.

[0149] The preparation method of the foam is the same as that of Example 1, and a finished foam HSN3 is obtained.

[0150] Comparative Example 4

[0151] The formula of the foam provided in this comparative example is the same as that of Example 3.

[0152] Preparation method of foam: In step S2, the aging treatment is not divided into two stages, but a one-step aging treatment is adopted, the aging temperature is 50° C., the time is 18 min, and the remaining operations are the same as in Example 3, to obtain the finished foam TSN4.

[0153] Comparative Example 5

[0154] The formula of the foam provided in this comparative example is the same as that of Example 3.

[0155] Preparation method of foam: In step S2, the aging treatment is not divided into two stages, but a one-step aging treatment is adopted, the aging temperature is 75° C., the time is 18 min, and the remaining operations are the same as those in Example 3, to obtain the finished foam TSN5.

[0156] Comparative Example 6

[0157] The formula of the foam provided in this comparative example is the same as that of Example 3.

[0158] Preparation method of foam: In step S2, the aging treatment is not divided into two stages, but a one-step aging treatment is adopted, the aging temperature is 100° C., the time is 18 min, and the remaining operations are the same as in Example 3, to obtain the finished foam TSN6.

[0159] Comparative Example 7

[0160] 1) The foam provided in this comparative example includes, by weight, 19.15 parts of carboxylated modified HTPB (same as in Example 1), 16 parts of NJ-305, 56.75 parts of EP-3600, 1.66 parts of silicone, 0.04 parts of stannous octoate, 4.6 parts of triethanolamine, 0.3 parts of deionized water, 1.5 parts of color paste and 27 parts of diphenylmethane diisocyanate MDI-50.

[0161] 2) The preparation method of the foam comprises the following steps:

[0162] S1. Mix the carboxylated modified HTPB, NJ-305, EP-3600, silicone, stannous octoate, triethanolamine, water and color paste according to the above-mentioned parts to obtain mixed material A;

[0163] S2. Mix the mixed material A with diphenylmethane diisocyanate MDI-50, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 45°C for 8 minutes, and the second stage is high-temperature aging at a temperature of 95°C for 18 minutes to obtain polyurethane foam.

[0164] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0165] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam TSN7.

[0166] Comparative Example 8

[0167] 1) The foam provided in this comparative example includes, by mass, 18.22 parts of carboxylated modified HTPB (same as in Example 1), 17 parts of NJ-305, 57.74 parts of EP-3600, 1.78 parts of silicone, 0.06 parts of dibutyltin dilaurate, 2.96 parts of 1,4-butanediol, 0.34 parts of deionized water, 1.9 parts of color paste and 37 parts of diphenylmethane diisocyanate MDI-50.

[0168] 2) The preparation method of the foam comprises the following steps:

[0169] S1. Mix the carboxylated modified HTPB, NJ-305, EP-3600, silicone, dibutyltin dilaurate, 1,4-butanediol, water and color paste according to the above-mentioned parts to obtain mixed material A;

[0170] S2. Mix the mixed material A with diphenylmethane diisocyanate MDI-50, apply coating to the mixture through a coating machine, and perform aging treatment after coating to make it foamed. The aging treatment is divided into two stages, wherein the first stage is low-temperature aging at a temperature of 40°C for 7 minutes, and the second stage is high-temperature aging at a temperature of 100°C for 16 minutes to obtain polyurethane foam.

[0171] S3, performing a splitting process on the polyurethane foam to remove the epidermis on the surface of the foam to obtain skinless polyurethane foam.

[0172] S4. Surface treatment is performed on the skinless polyurethane foam. Polydimethylsiloxane is sprayed on the surface of the skinless polyurethane foam using a gravity-type physical and chemical spray gun. The spraying is repeated 3 times to obtain a finished foam TSN8.

[0173] Comparative Example 9

[0174] The formula of the foam provided in this comparative example is the same as that of Example 1.

[0175] The preparation method of the foam is the same as that of Example 1, except that the polyurethane foam is not subjected to a layer splitting treatment to obtain a finished foam CSN9.

[0176] Comparative Example 10

[0177] The formula of the foam provided in this comparative example is the same as that of Example 1.

[0178] The preparation method of the foam is the same as that of Example 1, except that polydimethylsiloxane is not sprayed on the surface of the skinless polyurethane foam to obtain the finished foam CSN10.

[0179] The foams prepared in the examples and comparative examples were tested for performance, and the testing method was as follows:

[0180] 1) Porosity and average pore size: Use a scanning electron microscope to observe the pore morphology inside the foam sample to obtain a microscopic SEM image, and use Nano Measure software to count the pore size and pore density (porosity) and calculate the average value. When counting, ensure that more than 200 pores are counted for each sample to ensure the accuracy of the data; the porosity refers to the percentage of the internal pore volume in the foam to the total foam volume, calculated according to the formula Φ = (1-ρ / ρ0) × 100%, where Φ is the porosity; ρ is the density of the foam material, the unit is kg / m 3 ; ρ0 is the density of the corresponding foam material matrix, in kg / m 3 (Polyurethane foam ρ0=1200kg / m 3 ).

[0181] 2) Saturated electrolyte adsorption rate: Use the weighing method to calculate the saturated electrolyte adsorption rate of the foam. Specifically: weigh the weight of the above foam (length, width and thickness are 5cm×5cm×1cm), record it as W0, and then completely immerse it in the electrolyte to ensure that the foam fully absorbs the electrolyte. After leaving it for 0.5h, 1h, 1.5h, and 2h, take it out and gently wipe the surface of the foam with filter paper to remove excess electrolyte. Weigh the weight of the foam after soaking in the electrolyte for different times, record it as W 0.5 , W1, W 1.5 , W2, calculate the electrolyte adsorption rate of the foam after soaking in the electrolyte for different time periods. For example, the electrolyte adsorption rate of the foam after soaking in the electrolyte for 0.5h is (W 0.5-W0) / W0. The electrolyte used in the test of this application is 1M LiPF6+EC / DMC (1:1) v / v, purchased from Nanjing Mojies Energy Technology Co., Ltd., product model MJS-LBE01-180101. The experiment found that the adsorption rate of the electrolyte of the above foams immersed in the electrolyte for 1h, 1.5h, and 2h is equal, that is, the adsorption rate of the electrolyte of the foam immersed in the electrolyte for 1h is the saturated adsorption rate of the electrolyte of the foam. The saturated adsorption rate of the electrolyte of the foams prepared in each embodiment and comparative example is listed in Table 3.

[0182] 3) Compression strength of foam under 25% compression deformation: Referring to ASTM D1056 standard, the foam is subjected to compression test using an electronic universal testing machine to test its stress value under 25% compression deformation.

[0183] 4) Compression strength decay rate of the foam after being soaked in electrolyte for 72 hours: The strength of the foam before being soaked in electrolyte was tested according to ASTM D 3574 (stress of the foam under 25% compression deformation), and then it was completely soaked in electrolyte for 72 hours, taken out and placed in a 100°C oven for drying for 30 minutes, and the compression strength of the foam after being soaked in electrolyte for 72 hours was tested. The strength change value before and after the foam was soaked in electrolyte was calculated, that is, the compression strength decay rate of the foam after being soaked in electrolyte for 72 hours was obtained. The purpose is to test the change in the compressive strength of the foam after the performance of the foam adsorbing electrolyte reaches the saturated electrolyte adsorption rate, and continue to soak in electrolyte, so as to evaluate the foam's resistance to electrolyte corrosion.

[0184] 5) Foam water absorption rate: refer to ASTM D1056 standard, place the foam underwater at a depth of 5 cm, soak it in water for 24 hours, then wipe it dry, calculate the weight change rate, and get the water absorption rate.

[0185] 6) Contact angle between foam and water: The contact angle between foam and water is measured by using an Attensionθ optical tensiometer, through direct observation, analysis and calculation of the shape of the liquid droplet formed on the solid surface, to obtain the value of the contact angle.

[0186] The performance test results of the hydrophobic foams prepared in Examples 1 to 9 are shown in Table 3.

[0187] Table 3 Properties of the hydrophobic foams obtained in Examples 1 to 9

[0188]

[0189] The test results show that the porosity of the hydrophobic foam prepared in Examples 1 to 9 of the present application is 60% to 85%, the average pore size of the foam is 0.25mm to 0.66mm, and the compressive strength under 25% compression deformation is 52KPa to 75KPa. The saturated electrolyte adsorption ratio of the above foam is 8.91g / g to 17.41g / g, and the compression strength attenuation rate of the foam after 72 hours of infiltration of the electrolyte is 3.36% to 8.61%, indicating that the foam has a strong ability to adsorb electrolyte and is resistant to electrolyte corrosion. The water absorption rate of the above foam is 10.27% to 15.25%, and the contact angle between the foam and water is 145.76° to 160.47°, indicating that the hydrophobic foam prepared in this application has an excellent hydrophobic effect, and its application between the bare battery cell and the cylindrical shell can play a role in waterproofing and moisture resistance.

[0190] It can be seen from Examples 1 to 4 and Examples 5 and 6 that the average pore size of foams PU-5 and PU-6 is significantly smaller than that of foams PU-1 to PU-4. The reason may be that Examples 1 to 4 only use one catalyst, and the gelation rate of the foam system is slow, which leads to a larger pore size in the foam. When two or more composite catalysts are used (such as Examples 5 and 6), the gelation rate of the foam system is faster, which leads to a smaller pore size in the foam.

[0191] The state of the foam HSN1 prepared in comparative example 1 after being soaked in electrolyte for 72 hours ( Figure 5 ), it can be seen that the morphology of the foam has changed significantly. When the foam is clamped with tweezers, the foam breaks. After testing, the compression strength decay rate of foam HSN1 after immersion in electrolyte for 72 hours is 80.23%, and the water absorption rate is 55.10%, which are significantly higher than those in Example 1. The contact angle between the foam and water is 112.8°, which is significantly lower than that in Example 1. The reason for the analysis may be that polyurethane foam is the reaction product of polyol and isocyanate. Carboxyl-modified hydroxyl-terminated polybutadiene is a polyolefin polyol with hydroxyl groups at both ends of the molecular chain. In Example 1, it is used as a raw material in the foaming reaction of polyurethane foam. The carboxyl group and the isocyanate group undergo a series reaction of acid-base reaction and nucleophilic addition. Through this reaction, a new carbon-nitrogen bond can be constructed to generate urea and isourea products, thereby improving the strength and toughness of the foam and significantly improving the situation that the foam is not resistant to electrolyte. At the same time, the segment structure of the carboxylated modified hydroxy-terminated polybutadiene does not contain polar ester groups and ether groups, and has the characteristics of excellent hydrolysis resistance, good low-temperature flexibility, chemical corrosion resistance and low surface energy. Introducing it into the polyurethane skeleton can improve the water repellency of the foam to a certain extent. However, the foam formula of Comparative Example 1 does not contain modified hydroxy-terminated polybutadiene, so that after the foam is soaked in the electrolyte for a long time, the foam strength is greatly reduced, it is very easy to break, and it is not resistant to electrolyte corrosion, and the water repellency is poor.

[0192] The compression strength decay rate of the foam HSN2 prepared in comparative example 2 after being soaked in electrolyte for 72 hours was only 3.48%, but the strength of the foam HSN2 before being soaked in electrolyte was poor, and the compression strength under 25% compression deformation was 32.87 KPa. The compression strength decay rate of the foam HSN3 prepared in comparative example 3 after being soaked in electrolyte for 72 hours was 16.87%. The reasons may be analyzed as follows: polyurethane is composed of soft segments and hard segments, and there is a microphase separation structure between the soft and hard segments of polyurethane; the polyolefin structure in the carboxylated modified HTPB molecular chain is a flexible structure. When the amount of carboxylated modified HTPB in the foam formula is low (the mass ratio of modified terminal hydroxyl polybutadiene and polyether polyol in Comparative Example 3 is 1:5.5), the soft segment region (the polyolefin structure in the carboxylated modified HTPB and the polyether phase region in the polyether polyol) can be relatively evenly blended, thereby improving the compressive strength of the foam, but the amount of modified HTPB added is too low to improve the foam's resistance to electrolyte corrosion; when the amount of modified HTPB in the foam formula is high (the mass ratio of modified terminal hydroxyl polybutadiene and polyether polyol in Comparative Example 2 is 1:2), due to the large difference in the flexibility of polyether polyol and modified HTPB, the copolymerization of the two is poor, resulting in an uneven structure of the foam, which increases the defects in the soft segment phase region, thereby reducing the compressive strength of the foam and failing to slow down battery expansion.

[0193] The porosity of the foams TSN4 to TSN6 prepared in Comparative Examples 4 to 6 is 26% to 31%, the average pore size is 008 to 0.15 mm, and the saturated electrolyte adsorption ratio is 4.28 to 5.12 g / g, which are significantly lower than that in Example 3. The reason for the analysis may be that the aging process in Comparative Examples 4 to 6 is a one-step aging process, while the embodiment adopts a two-stage aging process. The first stage is low-temperature aging, and the temperature is controlled at 50°C to 65°C. At this time, the strength and viscoelasticity of the polyurethane foam are extremely low, the surface tension is small, and the resistance to the growth of bubbles is small, which is conducive to the growth of bubbles, so that the foam has a higher porosity and a larger pore size. The second stage is high-temperature aging, and the temperature is controlled at 80°C to 100°C to ensure that the reaction is completely cured, so that the foam is fully matured and has a certain strength. The two-stage aging can effectively improve the porosity of the foam, increase the pore size, and thus improve the adsorption capacity of the foam to the electrolyte.

[0194] The compressive strengths of the foams TSN7 and TSN8 prepared in Comparative Examples 7 and 8 under 25% compression deformation are 28.17 KPa and 31.19 KPa, respectively, which are lower than those in the embodiments. The reason may be that the aging temperature in the first stage of Comparative Examples 7 and 8 is too low, less than 50°C, which increases the pore diameter of the foam during the aging and foaming process, resulting in poor pore forming and easy collapse, resulting in low compression strength of the foam.

[0195] The saturated electrolyte adsorption rate of the foam CSN7 prepared in Comparative Example 9 is 7.34 g / g, which is significantly lower than that in Example 1 (the saturated electrolyte adsorption rate is 17.41 g / g). The reason may be that in Example 1, the polyurethane foam is subjected to a layer-splitting treatment to remove the epidermis on the surface of the foam, so that the pores of the foam are exposed, and the electrolyte can more easily infiltrate the foam, thereby improving the foam's ability to adsorb the electrolyte; while in Comparative Example 9, the foam is not subjected to a layer-splitting treatment, and the upper and lower surfaces of the prepared foam CSN7 both have a relatively dense epidermis, which is not conducive to the electrolyte entering the interior of the foam, thereby reducing the saturated electrolyte adsorption rate of the foam.

[0196] The water absorption rate of the foam CSN8 prepared in Comparative Example 10 is 29.14%, and the contact angle between the foam and water is 68.13°. Compared with the foam PU-1 in Example 1, the hydrophobic effect of the foam CSN8 is poor. This may be because the surface roughness of the polyurethane foam is greatly improved after splitting. In Example 1, polydimethylsiloxane is attached to the surface of the rough structure as a low surface energy material, so that the skinless foam forms a hydrophobic surface, which is used between the bare battery cell and the cylindrical shell to play a role in waterproofing and moisture resistance. When preparing the hydrophobic foam in Comparative Example 10, polydimethylsiloxane is not sprayed on the surface of the skinless polyurethane foam, which causes the hydrophobic effect of the foam to deteriorate.

[0197] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A hydrophobic foam capable of absorbing electrolyte and resistant to electrolyte corrosion, characterized in that: The porosity of the hydrophobic foam is 60% to 85%, the average pore diameter is 0.25 mm to 0.66 mm, the saturated electrolyte adsorption rate is 8.91 g / g to 17.41 g / g, the water absorption rate is 10.27% to 15.25%, and the contact angle between the foam and water is 145.76° to 160.47°; The compressive strength of the hydrophobic foam under 25% compression deformation is 52KPa-75KPa, and the compressive strength attenuation rate after being soaked in electrolyte for 72 hours is 3.36%-8.61%.

2. The hydrophobic foam according to claim 1, characterized in that: Calculated by mass, it comprises 92 to 95 parts of polyol, 0.3 to 0.5 parts of foaming agent, 2 to 5 parts of cross-linking agent, 0.04 to 0.08 parts of catalyst, 1 to 2 parts of surfactant, 1 to 2 parts of color paste and 27 to 45 parts of isocyanate; The polyol comprises carboxylated modified hydroxyl-terminated polybutadiene and polyether polyol, and the mass ratio of the carboxylated modified hydroxyl-terminated polybutadiene to the polyether polyol is 1:(2.5-5).

3. The hydrophobic foam according to claim 2, characterized in that: The polyether polyol comprises a polyether polyol A having a hydroxyl value of 110 mg KOH / g to 450 mg KOH / g and a polyether polyol B having a hydroxyl value of 25 mg KOH / g to 56 mg KOH / g; When used in hydrophobic foam, the carboxylated modified hydroxy-terminated polybutadiene can enhance the water repellency, compression strength and electrolyte corrosion resistance of the foam.

4. The hydrophobic foam according to claim 3, characterized in that: The polyether polyol A is selected from one or more of NJ-305, PTMG, DL-1000D, DL-400, TMN-450, VORANOL T5001 and VORANOL CP450; The polyether polyol B is selected from one or more of EP-3600, DL-2000D, POP36 / 38, ZR-001, EP-330N, VORANOL4000LM and VORAPELD3201.

5. The hydrophobic foam according to claim 2, characterized in that: The foaming agent is water; The cross-linking agent is selected from at least one of glycerol, triethanolamine, 1,4-butanediol, ethylene glycol, 1,6-hexanediol, primary hydroxyl tetraol and bis-2-(hydroxypropyl)aniline; The catalyst is selected from at least one of an amine catalyst and an organic metal catalyst; The surfactant is silicone; The isocyanate is selected from modified diisocyanate with an isocyanate content of 30 wt % to 50 wt %.

6. The hydrophobic foam according to claim 5, characterized in that: The amine catalyst is one or more of triethylenediamine, bis(dimethylaminopropylamine)isopropyl alcohol, trimethylethanolamine, pentamethyldipropylenetriamine, dimethylethanolamine and trimethylhydroxyethylethylenediamine; The organometallic catalyst is selected from one or more of an organotin compound, an organobismuth compound and an organozinc compound; The modified diisocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate and isophorone diisocyanate.

7. The method for preparing the hydrophobic foam according to any one of claims 1 to 6, characterized in that: The steps include: S1. Mix the polyol, the blowing agent, the cross-linking agent, the catalyst, the surfactant and the color paste according to a ratio to obtain a mixed material A; S2, mixing the mixed material A and the isocyanate according to a ratio, and then applying them on the surface of the substrate, performing low-temperature aging and high-temperature aging to obtain a polyurethane foam; S3, splitting the polyurethane foam to remove the epidermis to obtain skinless polyurethane foam; S4, spraying polydimethylsiloxane on the surface of the skinless polyurethane foam to obtain a hydrophobic foam.

8. The preparation method according to claim 7, characterized in that: In step S1, the carboxylated modified hydroxyl-terminated polybutadiene is obtained by graft polymerization of hydroxyl-terminated polybutadiene and mercaptosuccinic acid.

9. The preparation method according to claim 7, characterized in that: In step S2, the low-temperature aging temperature is 50°C to 65°C, and the time is 5min to 8min; the high-temperature aging temperature is 80°C to 100°C, and the time is 10min to 20min.

10. A foam for filling the gap between a bare battery cell and a battery shell, characterized in that: The invention comprises the hydrophobic foam according to any one of claims 1 to 6.

Citation Information

Cited By

  • FLAMMABLE ELECTROLYTE VAPOR TRAPPER AND BATTERY PACK WITH FLAMMABLE ELECTROLYTE VAPOR TRAPPER

    DE102024103896A1