Halogen-free flame-retardant 5VA-grade polypropylene composite material as well as preparation method and application thereof

By using an NP-based intumescent flame retardant and a mixture of ethylene-cyclic olefin copolymer and low-density polyethylene in a specific weight ratio to form a dense char layer, the burn-through problem of halogen-free flame-retardant 5VA grade polypropylene material in combustion tests was solved, achieving halogen-free flame retardancy and anti-dripping effects, and avoiding environmental risks.

CN118931041AActive Publication Date: 2024-11-12JIANGSU KINGFA SCI & TECH ADVANCED MATERIALS CO LTD +1

Patent Information

Application Number
CN202411207475.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare halogen-free flame-retardant 5VA grade polypropylene materials, especially thin sheet materials which are prone to burn-through in combustion tests, and the addition of anti-dripping agents introduces PFAS substances with environmental risks.

Method used

A halogen-free flame-retardant 5VA grade polypropylene composite material was prepared by using an NP-based intumescent flame retardant and a mixture of ethylene-cyclic olefin copolymer and low-density polyethylene in a specific weight ratio as a flame retardant synergist to form a dense char layer, improve flame retardant efficiency, and reduce combustion shrinkage.

Benefits of technology

It achieves halogen-free flame retardant effect, solves the problem of burn-through in combustion tests of 5VA grade polypropylene composite materials, avoids environmental risks, and improves the anti-dripping performance of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005019430090000061
    Figure BDA0005019430090000061
  • Figure BDA0005019430090000071
    Figure BDA0005019430090000071
  • Figure BDA0005019430090000072
    Figure BDA0005019430090000072
Patent Text Reader

Abstract

The invention discloses a halogen-free flame-retardant 5VA-grade polypropylene composite material as well as a preparation method and application thereof, and relates to the technical field of modified plastic processing. The invention provides a halogen-free flame-retardant 5VA-grade polypropylene composite material. The halogen-free flame-retardant 5VA-grade polypropylene composite material comprises the following components in parts by weight: 50-60 parts of polypropylene resin, 25-35 parts of a flame retardant, 5-15 parts of a flame-retardant synergist, 0.1-0.5 part of an antioxidant and 0.1-0.5 part of a lubricant, wherein the flame retardant is an N-P intumescent flame retardant, the flame retardant synergist is a mixture of an ethylene-cycloolefin copolymer and low-density polyethylene, and the weight ratio of the ethylene-cycloolefin copolymer to the low-density polyethylene is greater than or equal to 1. According to the invention, the flame retardant and flame retardant synergist system with specific components and parts by weight is adopted to successfully replace PTFE (Polytetrafluoroethylene) with environmental protection risk, so that good halogen-free flame retardance and good anti-dripping effect are realized, and meanwhile, the problem of burnthrough caused by multiple times of flame application in a 5VA-grade polypropylene composite material square plate testing process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of modified plastic processing, in particular to a halogen-free flame-retardant 5VA grade polypropylene composite material and a preparation method and application thereof. Background Art

[0002] In 2023, the European Chemicals Agency published a draft restriction on per- and polyfluoroalkyl substances (PFAS). The PFAS in this restriction proposal is defined as any fluorinated chemical (except a few structures) that contains at least one perfluorinated methyl (CF3-) or methylene (-CF2-) carbon atom (without any H / Cl / Br / I). The main reason for the restriction is that PFAS is very persistent in the environment, and if not restricted, it will have a negative impact on human health and the environment. In the field of flame retardant modified plastics, polytetrafluoroethylene (PTFE) is a commonly used modification aid and can be used as an anti-dripping agent, especially for 5VA high flame retardant grade polypropylene materials, it is an indispensable component. Due to the complex composition and numerous types of perfluorinated compounds, PTFE will inevitably contain a small amount of PFAS restricted substances during the synthesis process.

[0003] Polypropylene material has a lower oxygen index and is more flammable than other engineering plastics, making it more difficult to modify to flame retardancy, especially for 5VA-level halogen-free flame retardant systems with a thickness of less than 2.0 mm. 5VA combustion requires testing both specimens and square plates. During the combustion test of the square plates of the polypropylene flame retardant system, an obvious "shrinkage" phenomenon will occur, causing the square plates to easily burn through and fail the test. Currently, the commonly used solutions are to add glass fiber, mineral fillers, thermal insulation agents, anti-drip agents, etc. The addition of fillers will significantly reduce the physical properties of the material. Although the addition of anti-drip agents can improve this problem to a certain extent, it cannot completely solve the problem and will introduce PFAS restricted substances.

[0004] Therefore, it is of great significance to develop a halogen-free flame retardant 5VA grade flame retardant polypropylene material. Summary of the invention

[0005] Based on this, the purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a halogen-free flame retardant 5VA grade flame retardant polypropylene material and a preparation method and application thereof.

[0006] To achieve the above-mentioned purpose, the technical scheme adopted by the present invention is: a halogen-free flame retardant 5VA grade polypropylene composite material, comprising the following components in parts by weight: 50-60 parts of polypropylene resin, 25-35 parts of flame retardant, 5-15 parts of flame retardant synergist, 0.1-0.5 parts of antioxidant, and 0.1-0.5 parts of lubricant; wherein the flame retardant is an NP-based intumescent flame retardant, and the flame retardant synergist is a mixture of ethylene-cycloolefin copolymer and low-density polyethylene, wherein the weight ratio of ethylene-cycloolefin copolymer to low-density polyethylene is ≥1.

[0007] The present invention successfully replaces PTFE with environmental risks through flame retardants and flame retardant synergist systems selected by specific components and weight parts, achieves good halogen-free flame retardancy and good anti-dripping effect, and solves the problem of burn-through caused by multiple flames during the test of 5VA grade polypropylene composite square plates. The flame retardant selected by the present invention is an NP series intumescent flame retardant, which belongs to the intumescent flame retardant mechanism. Combined with the flame retardant synergist system of specific components and weight parts, on the one hand, it can promote the formation of the carbon layer and increase the density of the carbon layer. The rapidly formed carbon layer can also effectively improve the firmness of the system, improve the flame retardant efficiency, and solve the problem of burn-through caused by multiple flames during the test of 5VA grade polypropylene composite square plates; on the other hand, it can reduce the shrinkage of the square plate during the combustion process, reduce the orientation and stress of the square plate during the molding and preparation process, and fundamentally solve the problem of burn-through caused by multiple flames during the test of halogen-free flame retardant 5VA grade polypropylene composite square plates.

[0008] The inventors found in actual experiments that the weight ratio of ethylene-cycloolefin copolymer and low-density polyethylene in the flame retardant synergist affects the combustion performance of the halogen-free flame retardant 5VA grade polypropylene composite material. When the weight ratio of ethylene-cycloolefin copolymer and low-density polyethylene in the flame retardant synergist is less than 1, the formation of the char layer is affected, and dripping and burn-through problems will occur during the combustion process.

[0009] Preferably, the ethylene-cycloolefin copolymer includes at least one of an ethylene-norbornene copolymer and an ethylene-tetracyclododecene copolymer.

[0010] Preferably, the weight percentage of the PP resin in the halogen-free flame-retardant 5VA grade polypropylene composite material is not less than 45%.

[0011] Optionally, the weight of the PP resin is in the range of 50, 51, 53, 55, 58, 60 parts or any two of them; the weight of the flame retardant is in the range of 25, 28, 30, 32, 35 parts or any two of them; the weight of the flame retardant synergist is in the range of 5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 12, 15 parts or any two of them; the weight of the antioxidant is in the range of 0.1, 0.2, 0.3, 0.4, 0.5 parts or any two of them; the weight of the lubricant is in the range of 0.1, 0.2, 0.3, 0.4, 0.5 parts or any two of them.

[0012] Preferably, the ethylene-cycloolefin copolymer has a melt index of 10-30 g / 10 min at 260° C. and 2.16 kg according to ISO1133-2011, and the low-density polyethylene has a melt index of 0.2-5 g / 10 min at 190° C. and 2.16 kg according to ISO1133-2011.

[0013] Optionally, the melt index of the ethylene-cycloolefin copolymer at 260°C and 2.16 kg according to ISO1133-2011 is one of or any two of 10 g / 10 min, 12 g / 10 min, 15 g / 10 min, 20 g / 10 min, 22 g / 10 min, 23 g / 10 min, 25 g / 10 min, 28 g / 10 min, and 30 g / 10 min. Optionally, the low density polyethylene has a melt index of 0.2 g / 10 min, 0.5 g / 10 min, 1 g / 10 min, 2 g / 10 min, 2.5 g / 10 min, 3 g / 10 min, 3.5 g / 10 min, 4 g / 10 min, 4.5 g / 10 min, 4.8 g / 10 min, 5 g / 10 min or any two of the range values ​​at 190 ° C and 2.16 kg according to ISO1133-2011.

[0014] Preferably, the weight ratio of the ethylene-cycloolefin copolymer to the low-density polyethylene is (5-7):(3-5). Further preferably, the weight ratio of the ethylene-cycloolefin copolymer to the low-density polyethylene is (5-6):5.

[0015] The inventors found in actual experiments that the weight ratio of ethylene-cycloolefin copolymer and low-density polyethylene in the flame retardant synergist will further affect the combustion performance of the halogen-free flame retardant 5VA grade polypropylene composite material. When the weight ratio of ethylene-cycloolefin copolymer and low-density polyethylene is (5-6):5, it is more conducive to the formation of the carbon layer, and the flame retardant effect of the prepared polypropylene composite material is better.

[0016] Preferably, the polypropylene resin is at least one of homopolymer polypropylene, block copolymer polypropylene and random copolymer polypropylene, and the polypropylene has a melt index of 0.5-30 g / 10 min at 230° C. and 2.16 kg according to ISO1133-2011.

[0017] Optionally, the melt index of the polypropylene at 230° C. and 2.16 kg according to ISO 1133-2011 is 0.5 g / 10 min, 1 g / 10 min, 2 g / 10 min, 2.5 g / 10 min, 3 g / 10 min, 3.5 g / 10 min, 4 g / 10 min, 4.5 g / 10 min, 4.8 g / 10 min, 5 g / 10 min, 7 g / 10 min, 9 g / 10 min, 10 g / 10 min, 12 g / 10 min, 15 g / 10 min, 20 g / 10 min, 22 g / 10 min, 23 g / 10 min, 25 g / 10 min, 28 g / 10 min, or 30 g / 10 min, or any two of the range values.

[0018] Preferably, the NP-based intumescent flame retardant is at least one of pyrophosphate piperazine, ammonium polyphosphate, and triazine carbon-forming agents; and / or the antioxidant is at least one of hindered phenol antioxidants and phosphite antioxidants; and / or the lubricant is at least one of stearates, stearic acid esters, and ethylene bisstearamide.

[0019] Optionally, the NP-based intumescent flame retardant includes piperazine pyrophosphate, ammonium polyphosphate, tris(phosphaphenanthrene-(hydroxymethyl)phenoxy) 1,3,5 triazine, poly(4,6-dichloro-N-butyl-1,3,5 triazine-2-amino-ethylenediamine), 2,4-diamino-6-hydroxyethylamino-1,3,5 triazine, and the like.

[0020] Optionally, the antioxidant includes antioxidant 168 (tris[2,4-di-tert-butylphenyl]phosphite), antioxidant 1010 (pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), and the like.

[0021] Optionally, the lubricant includes pentaerythritol stearate, zinc stearate, calcium stearate, and the like.

[0022] In addition, the present invention provides a method for preparing the halogen-free flame-retardant 5VA grade polypropylene composite material, comprising the following steps: uniformly mixing the components, melt-extruding and granulating to obtain the halogen-free flame-retardant 5VA grade polypropylene composite material.

[0023] Preferably, the temperature of the melt extrusion is 180-200° C., and the screw speed is 300-450 rpm.

[0024] Furthermore, the present invention provides the use of the halogen-free flame-retardant 5VA grade polypropylene composite material in the preparation of household appliances and electronic appliances. Specifically, the present invention provides the use of the halogen-free flame-retardant 5VA grade polypropylene composite material in the preparation of electric control boxes, motor housings, and air conditioner handles.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention successfully replaces PTFE with environmental risks through flame retardants and flame retardant synergist systems selected by specific components and weight parts, achieves good halogen-free flame retardancy, and good anti-dripping effect, and at the same time, solves the problem of burning through caused by multiple flames during the test of 5VA grade polypropylene composite square plates. The flame retardant selected by the present invention is an NP series intumescent flame retardant, which belongs to the intumescent flame retardant mechanism. Combined with the flame retardant synergist system of specific components and weight parts, on the one hand, it can promote the formation of the carbon layer and increase the density of the carbon layer. The rapidly formed carbon layer can also effectively improve the firmness of the system, improve the flame retardant efficiency, and solve the problem of burning through caused by multiple flames during the test of 5VA grade polypropylene composite square plates; on the other hand, it can reduce the shrinkage of the square plate during the combustion process, reduce the orientation and stress of the square plate during the molding and preparation process, and fundamentally solve the problem of burning through caused by multiple flames during the test of halogen-free flame retardant 5VA grade polypropylene composite square plates. DETAILED DESCRIPTION

[0026] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. Its purpose is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Unless otherwise specified, the experimental reagents and instruments designed for the implementation and comparative examples of the present invention are all commonly used ordinary reagents and instruments, which can be obtained from commercial channels. In the implementation and comparative examples, the experimental methods used are conventional methods unless otherwise specified; and unless otherwise specified, the raw materials used in parallel experiments are the same batch of raw materials.

[0027] The raw materials used in the embodiments and comparative examples are described below, but are not limited to these materials:

[0028] PP-1: HP500N, homopolymer polypropylene, melt index 12g / 10min (230℃, 2.16kg), CNOOC Shell Company;

[0029] PP-2: K8003, block copolymer polypropylene, melt index 3.0g / 10min (230℃, 2.16kg), Yangzi Petrochemical Company;

[0030] PP-3: PPH-Y26, homopolymer polypropylene, melt index 25g / 10min (230℃, 2.16kg), Zhenhai Refining and Chemical Company;

[0031] Flame retardant-1: a mixture of ammonium polyphosphate and tris(phosphaphenanthrene-(hydroxymethyl)-phenoxy)-1,3,5-triazine (SR-207), with a weight ratio of 5:1, commercially available;

[0032] Flame retardant-2: piperazine pyrophosphate, commercially available;

[0033] Flame retardant-3: a mixture of octabromo-S-ether and antimony trioxide, with a weight ratio of 12:4, commercially available;

[0034] Ethylene-cycloolefin copolymer-1: ethylene-tetracyclododecene copolymer, APL6013T, melt index 15g / 10min (260℃, 2.16kg), Mitsui Co., Ltd., Japan;

[0035] Ethylene-cycloolefin copolymer-2: ethylene-tetracyclododecene copolymer, APL6011T, melt index 26g / 10min (260℃, 2.16kg), Mitsui Co., Ltd., Japan;

[0036] Ethylene-cycloolefin copolymer-3: ethylene-tetracyclododecene copolymer, APL6015T, melt index 10g / 10min (260℃, 2.16kg), Mitsui Co., Ltd., Japan;

[0037] Ethylene-cycloolefin copolymer-4: ethylene-norbornene copolymer, TOPAS 9506F-04, melt index 18 g / 10 min (260° C., 2.16 kg);

[0038] Cyclic olefin homopolymer-1: ZEONEX 350R, melt index 26g / 10min (260℃, 2.16kg), Zeon Co., Ltd., Japan;

[0039] Low-density polyethylene-1: LDPE 2426H, melt index 2.0g / 10min (190℃, 2.16kg), CNOOC Shell Company;

[0040] Low-density polyethylene-2: LDPE LD165, melt index 0.3g / 10min (190℃, 2.16kg), Yanshan Petrochemical Company;

[0041] Low-density polyethylene-3: LDPE 2426K, melt index 4.0g / 10min (190℃, 2.16kg), Maoming Petrochemical Company;

[0042] Linear low-density polyethylene: LLDPE 7042, melt index 2.0g / 10min (190℃, 2.16kg), Zhenhai Refining and Chemical Company;

[0043] High-density polyethylene: HDPE 5000S, melt index 1.0g / 10min (190℃, 2.16kg), Dushanzi Petrochemical;

[0044] Anti-dripping agent: polytetrafluoroethylene, commercially available;

[0045] Antioxidant: Antioxidant 1010 (tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl), commercially available;

[0046] Lubricant: calcium stearate, commercially available;

[0047] Examples 1-14 and Comparative Examples 1-8

[0048] The components of the halogen-free flame-retardant 5VA grade polypropylene composite material of the present invention are shown in Table 1 and Table 2. The preparation method of the halogen-free flame-retardant 5VA grade polypropylene composite material comprises the following steps: uniformly mixing the components, melt-extruding and granulating to obtain the halogen-free flame-retardant 5VA grade polypropylene composite material; wherein the melt-extrusion condition is: the screw speed is 400 rpm. The temperature of zone 1 is 180°C, the temperature of zones 2 to 6 is 190°C, the temperature of zones 7 to 10 is 200°C, and the temperature of zone 11 is 190°C.

[0049] Table 1

[0050]

[0051]

[0052] Table 2

[0053]

[0054] Table 3

[0055]

[0056]

[0057] Performance Testing

[0058] Test process: The flame retardant performance of the halogen-free flame retardant 5VA grade polypropylene composite material prepared in the above specific embodiments and comparative examples was tested according to the UL-94-2006 standard. The test samples were prepared by injection molding, wherein the thickness of the burning specimen was 1.5 mm and the size of the square plate was 150 mm × 150 mm × 1.5 mm.

[0059] Test performance parameters: The material can reach 5VA level only when both the specimen and the sample meet the combustion test.

[0060] (1) Vertical burning test, record the flame retardancy level according to the burning standard.

[0061] (2) 5VA specimen test: record whether the test is passed according to the combustion standard. If the test is passed, record the average value of the flame and flameless time (seconds) of the three specimens after the fifth ignition. In addition, record whether the absorbent cotton is ignited.

[0062] (3) 5VA sample test: record whether the sample is burned through according to the combustion standard.

[0063] Test results: as shown in Table 4.

[0064] Table 4

[0065]

[0066]

[0067] It can be seen from the above table that the polypropylene composite materials prepared in the embodiments of the present invention can all pass the 5VA test, which fundamentally solves the burn-through problem caused by multiple flame applications in the test of the halogen-free flame retardant 5VA grade polypropylene composite square plate.

[0068] From the comparison of Examples 1-10, it can be seen that when the flame retardant used in the polypropylene composite material is an NP-based intumescent flame retardant, the flame retardant synergist is a mixture of ethylene-cycloolefin copolymer and low-density polyethylene, the weight ratio of ethylene-cycloolefin copolymer to low-density polyethylene is ≥1, the melt index of the polypropylene resin is 0.5-30g / 10min, and the NP-based intumescent flame retardant, a polypropylene composite material that passes the 5VA test can be obtained.

[0069] By comparing Example 1 and Examples 11-14, it can be seen that when the weight ratio of the ethylene-cycloolefin copolymer to the low-density polyethylene is (5-7): (3-5), under the premise of passing the 5VA test, the average value of the flame and flameless time of the 1.5mm / 5VA-strip is ≤3.5 seconds, which is more conducive to the formation of the carbon layer, and the flame retardant effect of the prepared polypropylene composite material is better.

[0070] From the comparison of Example 1 and Comparative Examples 1-8, it can be seen that the flame retardant and flame retardant synergist system selected by specific components and weight parts in the present invention achieves a good anti-dripping effect under the synergistic effect of ethylene-cycloolefin copolymer and low-density polyethylene, successfully replaces PTFE with environmental risks, and achieves fluorine-free flame retardancy. In addition, it can effectively reduce the orientation and stress in the square plate forming preparation process, and fundamentally solve the burn-through problem caused by combustion shrinkage during the test process of the flame-retardant polyolefin material 5VA square plate.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A halogen-free flame-retardant 5VA grade polypropylene composite material, characterized in that: The invention comprises the following components in parts by weight: 50-60 parts of polypropylene resin, 25-35 parts of flame retardant, 5-15 parts of flame retardant synergist, 0.1-0.5 parts of antioxidant and 0.1-0.5 parts of lubricant; wherein the flame retardant is an NP-based intumescent flame retardant, and the flame retardant synergist is a mixture of ethylene-cycloolefin copolymer and low-density polyethylene, wherein the weight ratio of ethylene-cycloolefin copolymer to low-density polyethylene is ≥1.

2. The halogen-free flame-retardant 5VA grade polypropylene composite material according to claim 1, characterized in that: The ethylene-cycloolefin copolymer has a melt index of 10-30 g / 10 min at 260° C. and 2.16 kg according to ISO1133-2011, and the low-density polyethylene has a melt index of 0.2-5 g / 10 min at 190° C. and 2.16 kg according to ISO1133-2011.

3. The halogen-free flame-retardant 5VA grade polypropylene composite material according to claim 1, characterized in that: The weight ratio of the ethylene-cycloolefin copolymer to the low-density polyethylene is (5-7):(3-5).

4. The halogen-free flame-retardant 5VA grade polypropylene composite material according to claim 1, characterized in that: The polypropylene resin is at least one of homopolymer polypropylene, block copolymer polypropylene and random copolymer polypropylene. The polypropylene has a melt index of 0.5-30 g / 10 min at 230° C. and 2.16 kg according to ISO1133-2011.

5. The halogen-free flame-retardant 5VA grade polypropylene composite material according to claim 1, characterized in that: The NP-based intumescent flame retardant is at least one of piperazine pyrophosphate, ammonium polyphosphate, and triazine carbon formers; And / or, the antioxidant is at least one of a hindered phenol antioxidant and a phosphite antioxidant; And / or, the lubricant is at least one of stearates, stearic acid esters, and ethylene bis stearamide.

6. A method for preparing the halogen-free flame-retardant 5VA grade polypropylene composite material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: uniformly mixing the components, performing melt extrusion and granulation to obtain the halogen-free flame-retardant 5VA grade polypropylene composite material.

7. Use of the halogen-free flame-retardant 5VA grade polypropylene composite material as claimed in any one of claims 1 to 5 in the preparation of household appliances and electronic appliances.

8. Use of the halogen-free flame-retardant 5VA grade polypropylene composite material as claimed in any one of claims 1 to 5 in the preparation of an electric control box, a motor housing and an air conditioner handle.

Citation Information

Patent Citations

  • High-transparency and flame-retardant PP (polypropylene) / COC (cycloolefin copolymer) composite and preparation method thereof

    CN106700235A

  • High-rigidity low-opening-force cover material and preparation method and application

    CN107383583A

  • High-welding-strength polypropylene composition as well as preparation method and application thereof

    CN112094472A

  • Polyolefinic resin composition

    JP2001002860A

Cited By

  • Polypropylene-based, glass fiber reinforced, halogen-free flame retardant material compositions based on pcr

    CN122790337A