Wave-absorbing prepreg as well as preparation method and application thereof
Through the combination of solvent-free epoxy resin and graphene, carbon black, and carbon nanotubes, combined with hot melt infiltration and hot pressing curing processes, the problem of uneven solvent residue and absorbent distribution in the absorbent prepreg is solved, and the problem of uneven distribution of the absorbent is achieved. It improves wave absorption and mechanical properties, and is suitable for mass production.
Patent Information
- Application Number
- CN202410980076.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Solvent residues in the existing absorbing prepreg preparation process lead to environmental pollution and degradation of material properties, and uneven distribution of absorbing agent leads to poor absorption stability.
Solvent-free epoxy resin, graphene, carbon black and carbon nanotubes are used as absorbers, and the mixed solution is dispersed through a three-roll rolling machine, and the glass fiber fabric is immersed in a two-step hot melting method, and the glass fiber fabric is solidified in combination with a hot press tank. The process is used to prepare the absorbent prepreg to ensure uniform distribution of the absorbent and viscosity control.
It improves wave absorption performance and mechanical properties, ensures wave absorption stability, simplifies the process flow, is suitable for mass production, and avoids the traditional coating spraying and grinding steps.
Smart Images

Figure CN118931106A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of wave absorbing materials, and in particular relates to a wave absorbing prepreg, a preparation method and application thereof. Background Art
[0002] In addition to relying on appearance design, radar stealth mainly uses absorbing coatings and absorbing structures that can absorb radar waves, weakening the scattering field so that no effective echo signal can be formed. In the process of stealth technology research, absorbing coatings and absorbing structures have become the most important means to improve stealth performance besides appearance stealth design.
[0003] Structural absorbing materials are usually made of resin / fiber reinforced composite materials as carriers and absorbents. It is a multifunctional composite material that can not only bear structural parts, but also has the advantages of light weight and high strength of composite materials. It can also absorb or transmit electromagnetic waves well. It has become an important development direction of current stealth materials. The commonly used process methods for the preparation of traditional composite prepregs are premixing and prepreg. The prepreg method is to store a certain viscosity of glue in a glue tank, stir it evenly, and then continuously dip the entire bundle of continuous reinforcing fibers in the glue tank and dry it to an appropriate viscosity.
[0004] However, in actual applications, it is found that the existing prepreg method has the following two disadvantages when preparing absorbing prepregs:
[0005] (1) Prepregs require solvents during impregnation, and it is difficult to completely remove them during subsequent processing, which will cause a certain degree of environmental pollution. In addition, the residual solvent evaporates during material molding, which easily forms pores inside the material, thereby affecting the performance of the composite material;
[0006] (2) During the preparation of prepregs, the absorber powder used has a higher density than the matrix material, and has poor dispersibility when preparing the solution, and is easy to settle, resulting in uneven distribution of the absorbing component in the prepreg and poor absorbing stability. Summary of the invention
[0007] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a wave-absorbing prepreg, a preparation method and an application thereof, which have excellent mechanical and wave-absorbing properties and strong wave-absorbing stability.
[0008] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a wave-absorbing prepreg, which is composed of a resin, an absorbent and a glass fiber fabric; the absorbent is composed of graphene: carbon black: carbon nanotubes in a ratio of 50 to 120 parts: 5 to 45 parts: 10 to 30 parts; the total mass of the graphene, carbon black and carbon nanotubes accounts for 0.5% to 15% of the mass of the resin.
[0009] Furthermore, the resin is a solvent-free epoxy resin.
[0010] A method for preparing a microwave absorbing prepreg comprises the following steps:
[0011] S1, adding graphene, carbon black and carbon nanotubes to the resin, and dispersing them through a three-roll mill to form a mixed solution;
[0012] S2, hot-pressing and impregnating the glass fiber fabric and the mixed solution through a hot-melt two-step method to obtain a microwave absorbing prepreg;
[0013] S3, rolling up to obtain the finished microwave absorbing prepreg.
[0014] Furthermore, the glass fiber fabric is made of S-glass fiber and adopts a 1×1 plain weave form, and the fabric surface density is 60±5g / m 2 , the impregnation temperature is 80~150℃, the hot pressing pressure is 8~10kg / m 2 Woven.
[0015] Furthermore, the curing process of the absorbing prepreg in an autoclave requires a vacuum degree of not less than 0.085 MPa, the temperature is raised to 120° C. at 1-3° C., kept warm for at least 180 minutes, and then cooled to below 60° C. at 1-3° C. / min for demolding to obtain the absorbing composite material.
[0016] A microwave absorbing composite material using microwave absorbing prepregs, comprising a glass fiber prepreg layer, a microwave absorbing prepreg layer and a carbon fiber prepreg layer arranged in sequence from top to bottom; the thickness of the glass fiber prepreg layer is ≥0.3mm, the thickness of the carbon fiber prepreg layer is ≥0.6mm, and the thickness of the microwave absorbing prepreg layer is ≥2mm.
[0017] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:
[0018] (1) The absorbing prepreg of the present invention has no effect on its mechanical properties if the amount of absorbent added is not high. The resin and the absorbent can be fully impregnated into the glass fiber fabric, so that the uniformity of the absorbent is improved, thereby improving the absorbing performance;
[0019] (2) The microwave absorbing prepreg of the present invention ensures the viscosity of the mixed solution after the resin and the absorbent are mixed by controlling the temperature and the addition ratio, so that the absorbent can be suspended in the mixed solution and the absorbent is difficult to settle, thereby ensuring that the absorbent is evenly distributed in the prepreg;
[0020] (3) The absorbing composite material of the present invention realizes the integration of structural load-bearing and absorbing functions. The absorbing prepreg can be used to prepare absorbing structural parts of different specifications through a hot pressing process. The laying process is the same as that of conventional glass fiber prepreg, and the construction is convenient;
[0021] (4) The microwave-absorbing composite material prepared by the present invention can be formed in an integrated manner, eliminating the repeated spraying, grinding and repairing steps of traditional microwave-absorbing coatings, is more suitable for mass production, and can ensure process stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The technical solution of the present invention is further described below in conjunction with the accompanying drawings:
[0023] Figure 1 Schematic diagram of the preparation process of the microwave absorbing prepreg in one embodiment of the present invention;
[0024] Figure 2 This is a schematic structural diagram of a wave-absorbing composite material according to an embodiment of the present invention;
[0025] Figure 3 This is a schematic structural diagram of a second wave-absorbing composite material according to an embodiment of the present invention;
[0026] Figure 4 is a tensile performance diagram of the wave-absorbing composite material of the present invention;
[0027] Figure 5 is a bending performance diagram of the wave-absorbing composite material of the present invention;
[0028] Figure 6 is a compression performance diagram of the wave-absorbing composite material of the present invention;
[0029] Figure 7 This is a schematic diagram of reflectivity at 2-18 GHz of Example 1 of the invention;
[0030] Figure 8 This is a schematic diagram of reflectivity at 2-18 GHz of Example 2 of the invention;
[0031] Among them: a glass fiber prepreg layer 1, a carbon fiber prepreg layer 2, and an absorbing prepreg layer 3. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0033] The invention discloses a wave absorbing prepreg, which is composed of resin, absorbent and glass fiber fabric; the absorbent is composed of graphene: carbon black: carbon nanotubes in a proportion of 50-120 parts: 5-45 parts: 10-30 parts; the total mass of the graphene, carbon black and carbon nanotubes accounts for 0.5%-15% of the mass of the resin.
[0034] based on Figure 1 The preparation method of a microwave absorbing prepreg of the present invention comprises the following steps: S1, adding graphene, carbon black and carbon nanotubes into a resin, and dispersing them through a three-roller roller to form a mixed solution; S2, hot-pressing and impregnating a glass fiber fabric and the mixed solution through a hot-melt two-step method to obtain a microwave absorbing prepreg; S3, rolling up to obtain a finished microwave absorbing prepreg.
[0035] The absorbent in the absorbing prepreg of the present invention not only improves the absorbing performance, but also has no effect on its strength, that is, mechanical properties. The resin and the absorbent can be fully impregnated into the glass fiber fabric, so that the uniformity of the absorbent is improved, thereby improving the absorbing performance.
[0036] Secondly, the viscosity of the mixed solution after the resin and absorbent are mixed is ensured by controlling the temperature and adding ratio, so that the absorbent can be suspended in the mixed solution and it is difficult for the absorbent to settle, thereby ensuring that the absorbent is evenly distributed in the prepreg. Specifically, when the proportion of the absorbent in the mixed solution is increased from 0.5% to 5%, the viscosity of the mixed solution can be effectively increased. The mixture can be mixed evenly when the temperature is not higher than 60°C, but exceeding 60°C will affect the resin, so the temperature during mixing is generally not more than 60°C.
[0037] See also Figures 4 to 6 The microwave absorbing composite material using the microwave absorbing prepreg in the present invention is composed of a glass fiber prepreg layer, a microwave absorbing prepreg layer and a carbon fiber prepreg layer which are sequentially arranged up and down.
[0038] Two embodiments are listed below for specific description.
[0039] Example 1
[0040] based on Figure 2 In this embodiment, a wave-absorbing composite material is composed of a wave-absorbing prepreg layer, a glass fiber prepreg layer and a carbon fiber prepreg layer, wherein the wave-absorbing prepreg layer is composed of epoxy resin, graphene, carbon black, carbon nanotubes and glass fiber fabric, the mass ratio of graphene: carbon black: carbon nanotubes is 30:15:20, and the total mass of the carbon material is 10% of the resin.
[0041] When preparing the absorbing composite material, 3 layers of carbon fiber prepreg are used as the bottom layer with a thickness of about 0.4-0.5 mm, 8 layers of absorbing prepreg are used as the middle layer with a thickness of about 1.8 mm, and 8 layers of glass fiber prepreg are used as the surface layer with a thickness of about 0.6-0.8 mm. Then, they are autoclaved and cured to form a 30 cm×30 cm composite material sample with a thickness of about 2.8 mm.
[0042] The tensile strength of the wave-absorbing composite material prepared by the present invention is shown in the following table.
[0043]
[0044] Its bending strength is shown in the following table.
[0045]
[0046]
[0047] Its compressive strength is shown in the following table.
[0048] width thickness Maximum force Compression strength Compression modulus Failure strain Elastic modulus unit mm mm kN MPa GPa GPa Sample 1 11.83 3.13 12.42 335 0.0 0 0.0 Sample 2 12.08 2.82 10.72 315 0.0 0 0.0 Sample 3 11.83 3.16 11.62 311 0.0 0 0.0 Sample 4 11.92 2.98 12.16 342 0.0 0 0.0 Sample 5 11.88 3.09 10.62 289 0.0 0 0.0 Sample 6 11.92 2.9 10.83 313 0.0 0 0.0 average value 11.91 3.01 11.39 318 0.0 0 0.0 Standard deviation (n) 0.08 0.12 0.71 17 0.0 0 0.0 Coefficient of variation (%) 0.71 4.12 6.27 5 -1.$ -1 -1.$
[0049] In addition, the radar reflectivity of this embodiment at 2 to 18 GHz is as follows: Figure 7 shown.
[0050] In summary, in Example 1, the overall tensile strength of the absorbing composite material is about 389 MPa, the bending strength is 747 MPa, and the compressive strength is 318 MPa. By introducing carbon fiber prepreg into the glass fiber prepreg ply and performing structural configuration design, the structural absorbing performance and load-bearing performance are greatly enhanced, providing a new solution for the integrated design of lightweight, stealth and load-bearing of aircraft skins.
[0051] Example 2
[0052] based on Figure 3 The difference between this embodiment and the first embodiment is that the plying order of each prepreg layer is different when preparing the absorbing composite material. In this embodiment, 5 layers of carbon fiber prepreg are used as the bottom layer with a thickness of about 0.4-0.5 mm, followed by 3 layers of absorbing prepreg with a thickness of about 0.6-0.8 mm, 3 layers of glass fiber prepreg with a thickness of about 0.2-0.3 mm, 3 layers of absorbing prepreg with a thickness of about 0.6-0.8 mm, and 5 layers of glass fiber prepreg with a thickness of about 0.4-0.5 mm. The composite material sample of 30 cm×30 cm with a thickness of about 2.8 mm is formed by autoclave curing.
[0053] The reflectivity test results of the finally prepared wave-absorbing composite material are as follows: Figure 8 shown.
[0054] As described above, the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A microwave absorbing prepreg, characterized in that: The wave absorbing prepreg is composed of resin, absorbent and glass fiber fabric; the absorbent is composed of graphene: carbon black: carbon nanotubes in a proportion of 50-120 parts: 5-45 parts: 10-30 parts; the total mass of the graphene, carbon black and carbon nanotubes accounts for 0.5%-15% of the mass of the resin.
2. The microwave absorbing prepreg according to claim 1, characterized in that: The resin is a solvent-free epoxy resin.
3. A method for preparing the microwave absorbing prepreg according to claim 1, characterized in that: The steps include: S1, adding graphene, carbon black and carbon nanotubes to the resin, and dispersing them through a three-roll mill to form a mixed solution; S2, hot-pressing and impregnating the glass fiber fabric and the mixed solution through a hot-melt two-step method to obtain a microwave absorbing prepreg; S3, rolling up to obtain the finished microwave absorbing prepreg.
4. The process for preparing the microwave absorbing prepreg according to claim 3, characterized in that: The glass fiber fabric is made of S-glass fiber and adopts a 1×1 plain weave form. The fabric surface density is 60±5g / m 2 , the impregnation temperature is 80~150℃, the hot pressing pressure is 8~10kg / m 2 Woven.
5. The process for preparing the wave absorbing composite material according to claim 3, characterized in that: The curing process of the wave-absorbing prepreg in an autoclave requires a vacuum degree of not less than 0.085 MPa, and the temperature is raised to 120° C. at 1-3° C., kept warm for at least 180 minutes, and then cooled to below 60° C. at 1-3° C. / min to remove the film to obtain the wave-absorbing composite material.
6. A microwave absorbing composite material using a microwave absorbing prepreg, characterized in that: It comprises a glass fiber prepreg layer, a wave absorbing prepreg layer and a carbon fiber prepreg layer which are arranged in sequence from top to bottom; the thickness of the glass fiber prepreg layer is ≥0.3mm, the thickness of the carbon fiber prepreg layer is ≥0.6mm, and the thickness of the wave absorbing prepreg layer is ≥2mm.
Citation Information
Cited By
Resistive film, broadband wave-absorbing material and preparation method of broadband wave-absorbing material
CN121528667A