Special master batch for degradable foaming shoe material and preparation method thereof
By using modified talc powder and starch in polylactic acid masterbatches, combined with surface modifiers and other components, the problems of uneven dispersion and poor compatibility of talc powder during high content filling are solved, and efficient biodegradation is achieved and environmentally friendly shoe masterbatches reduce costs and improve material performance.
Patent Information
- Application Number
- CN202411266473.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional plastic slippers are difficult to degrade after use, resulting in environmental pollution. The high cost of polylactic acid limits its large-scale application in disposable slippers. There are problems of uneven dispersion and poor compatibility when filling with high content.
Using a combination of polylactic acid, starch, talc, surface modifier, plasticizer, stabilizer and antioxidant, the talc and starch are modified to form an excellent pore-forming agent, which improves its in PLA resin Dispersibility and compatibility, improve foaming ratio and porosity.
The high filling and uniform dispersion of talc powder in the PLA masterbatch is achieved, which improves the biodegradability and processing performance of the material, reduces costs, and reduces the pollution of the processing aids to the environment.
Smart Images

Figure CN118931137A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of degradable masterbatches, and in particular to a masterbatch special for degradable foaming shoe materials and a preparation method thereof. Background Art
[0002] With the advancement of urbanization and the rapid development of tourism, disposable slippers have good growth potential. However, traditional plastic slippers mostly use high molecular polymers made from non-renewable petroleum resources such as polyethylene (PE) and EVA, and they are almost indecomposable in the natural environment after use, generating a large amount of white pollution. After incineration, a large amount of toxic and harmful substances will be generated, bringing immeasurable pressure to the environment and resources. Problems such as shortage of petroleum resources and white pollution caused by plastic products are becoming increasingly serious.
[0003] Biodegradable plastics refer to plastics that can be degraded into carbon dioxide or / and methane, water and other inorganic salts by microorganisms in nature (such as soil or sand conditions) or under specific conditions (such as composting / anaerobic digestion conditions / aqueous culture medium). Therefore, the application of biodegradable materials can reduce the pollution caused by traditional polymer plastics to the environment. Polylactic acid (PLA) has good biodegradability and good mechanical properties, and is considered to be the most environmentally friendly polymer material with the most industrial prospects. The application of polylactic acid foaming shoe material masterbatch in disposable shoe materials has obvious advantages, which can not only reduce the amount and cost of materials, but also improve the performance of materials. As an environmentally friendly polymer material, it has a broad application space. However, the current price of polylactic acid is about 2 to 5 times the cost of polymers such as PE and polypropylene (PP), which limits its large-scale application in disposable slippers. Therefore, degradable plastics are often used in combination with low-cost filling materials (calcium carbonate, talcum powder and other inorganic non-metallic mineral materials or starch, fiber), etc. The resulting composite material can not only reduce costs, but also improve the processing performance of materials.
[0004] Talc is widely used as a low-cost filling material, but when filled with high content, there are technical problems such as uneven dispersion, poor compatibility with the substrate, and poor foaming ratio and pores in the degradation material. Therefore, it is urgent to provide a method that can achieve high filling of talc in PLA masterbatch without affecting compatibility. Summary of the invention
[0005] The purpose of the present invention is to provide a masterbatch for degradable foaming shoe materials and a preparation method thereof, so as to solve the problems of uneven dispersion of talc powder when filled with high content, poor compatibility with substrates, and improve the foaming ratio of degradable materials and unclear pores.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a masterbatch for degradable foaming shoe materials, comprising the following raw materials in parts by weight:
[0008] 40-70 parts of polylactic acid, 10-20 parts of starch, 30-50 parts of talc, 0.4-1.4 parts of surface modifier, 0.16-11.2 parts of plasticizer, 0.5-2.8 parts of stabilizer, 0.3-0.5 parts of antioxidant;
[0009] The surface modifier is one or more of isopropoxy tris(dioctyl phosphate) titanate, isopropyl tris(dodecylbenzenesulfonyl) titanate and bis(dioctyl pyrophosphate) ethylene titanate.
[0010] Preferably, in the masterbatch for biodegradable foaming shoe materials, the starch is one or more of corn starch, potato starch, and cassava starch, and the average particle size of the starch is 15 to 20 μm.
[0011] Preferably, in the masterbatch specially made for biodegradable foaming shoe materials, the specifications of the talcum powder are as follows: D50 is 3 to 5 μm, the silicon content is 40 to 45%, and the whiteness is 91 to 94 degrees.
[0012] Preferably, in the above-mentioned masterbatch for degradable foaming shoe materials, the plasticizer is one or more of plant oil degradable epoxy methyl ester, acetylated castor oil methyl ester, polyglycerol ester, N,N'-ethylene bisstearamide; the stabilizer is one or more of octadecanoic acid calcium salt, octadecanoic acid zinc salt, and octadecanoic acid barium salt.
[0013] Preferably, in the masterbatch for biodegradable foaming shoe materials, the antioxidant is tris(2,4-di-tert-butylphenyl)phosphite and / or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
[0014] The present invention also provides a method for preparing the special masterbatch for degradable foaming shoe materials, comprising the following steps:
[0015] (1) talcum powder, starch and a surface modifier are mixed and modified to obtain a mixture of modified talcum powder and starch;
[0016] (2) mixing the mixture of modified talcum powder and starch with polylactic acid, and then adding a plasticizer, a stabilizer, and an antioxidant to obtain a mixed material;
[0017] (3) Extruding and granulating the mixed material in turn to obtain a masterbatch for biodegradable foaming shoe material.
[0018] Preferably, in the method for preparing a masterbatch for biodegradable foaming shoe materials, when the modification temperature in step (1) is 120≤T≤150°C, the mixing speed in step (1) is 300-500r / min; when the modification temperature in step (1) is 150<T≤170°C, the mixing speed in step (1) is 180-260r / min;
[0019] The modification time in step (1) is 15 to 25 minutes.
[0020] Preferably, in the method for preparing a masterbatch for biodegradable foaming shoe materials, when the temperature of the mixture of modified talcum powder and starch and polylactic acid in step (2) is 100≤T≤120°C, the mixing speed is 100-200r / min; when the temperature of the mixture of modified talcum powder and starch and polylactic acid in step (2) is 80≤T<100°C, the mixing speed is 400-600r / min;
[0021] In step (2), the time for mixing the modified talcum powder, starch mixture and polylactic acid is 5 to 10 minutes.
[0022] Preferably, in the method for preparing the masterbatch for biodegradable foaming shoe materials, the rotation speed of adding the plasticizer, stabilizer and antioxidant and mixing in step (2) is 300-600 r / min, the temperature is 110-120° C., and the time is 3-5 min.
[0023] Preferably, in the method for preparing a special masterbatch for biodegradable foaming shoe materials, the process parameters of the extrusion granulation in step (3) are: extrusion temperature of 160-180°C, screw speed of 300-500r / min, melt pressure of 7-10MPa, and extrusion current of 70-80% of the rated current.
[0024] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The masterbatch for degradable foaming shoe materials obtained by the present invention is green, environmentally friendly and biodegradable: the masterbatch prepared by using biodegradable resin PLA as raw material and talcum powder as nucleating agent has a relative biodegradability rate of ≥60%; the inorganic powder originates from nature and eventually returns to nature, and will not cause any impact on the environment; the processing aids are preferably various esters and low molecular weight additives, and high molecular weight organic additives are excluded, thereby increasing the degradation rate of the product and reducing the pollution of the processing aids to the environment;
[0026] (2) The masterbatch for biodegradable foaming shoe materials obtained by the present invention has excellent foaming efficiency: the talc and starch treated with the surface modifier can improve their dispersibility and compatibility in the PLA resin, making them excellent pore-forming agents, improving the foaming ratio and pore gap of PLA;
[0027] (3) The present invention can improve the compatibility of inorganic / organic powders with biodegradable resins, improve their processing performance, improve the processing fluidity and plasticizing ability of materials in a screw extruder, and reduce the decomposition of biodegradable resins in the screw;
[0028] (4) The present invention also adds starch to improve the toughness of the material, while also achieving environmentally friendly degradation performance and increasing the degradation rate of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.
[0030] Figure 1 The present invention is a process flow chart for preparing a masterbatch specifically for degradable foamed shoe materials. DETAILED DESCRIPTION
[0031] The present invention provides a masterbatch for degradable foaming shoe materials, comprising the following raw materials in parts by weight:
[0032] 40-70 parts of polylactic acid, 10-20 parts of starch, 30-50 parts of talc, 0.4-1.4 parts of surface modifier, 0.16-11.2 parts of plasticizer, 0.5-2.8 parts of stabilizer, 0.3-0.5 parts of antioxidant;
[0033] The surface modifier is one or more of isopropoxy tris(dioctyl phosphate) titanate, isopropyl tris(dodecylbenzenesulfonyl) titanate and bis(dioctyl pyrophosphate) ethylene titanate.
[0034] In the present invention, the molecular weight of the polylactic acid is preferably 100-120, more preferably 100-110, and even more preferably 105.
[0035] In the present invention, the mass fraction of the polylactic acid is preferably 50 to 65 parts, more preferably 55 to 60 parts, and even more preferably 60 parts.
[0036] In the present invention, the starch is preferably one or more of corn starch, potato starch, and tapioca starch, more preferably one or two of corn starch and tapioca starch, and more preferably tapioca starch.
[0037] In the present invention, the average particle size of the starch is preferably 15 to 20 μm, more preferably 18 to 20 μm, and even more preferably 20 μm.
[0038] In the present invention, the molecular weight of the starch is preferably 5000-20000, more preferably 7000-12000, and even more preferably 8000-10000.
[0039] In the present invention, the mass fraction of the starch is preferably 10 to 16 parts, more preferably 10 to 12 parts, and more preferably 10 parts.
[0040] In the present invention, the specifications of the talc powder are preferably: D50 is 3-5μm, silicon content is 40-45%, and whiteness is 91-94 degrees; more preferably, D50 is 3.2-4.5μm, silicon content is 42-44%, and whiteness is 92-94 degrees; more preferably, D50 is 4.1μm, silicon content is 43%, and whiteness is 93 degrees.
[0041] In the present invention, the mass fraction of the talc is preferably 35 to 50 parts, more preferably 45 to 50 parts, and even more preferably 50 parts.
[0042] In the present invention, the surface modifier is one or more of isopropoxy tris(dioctyl phosphate) titanate (CAS: 65345-34-8), isopropyl tris(dodecylbenzene sulfonyl) titanate (CAS: 61417-55-8) and bis(dioctyl pyrophosphate) ethylene titanate (CAS: 65467-75-6), more preferably one or two of isopropyl tris(dodecylbenzene sulfonyl) titanate and bis(dioctyl pyrophosphate) ethylene titanate, more preferably two of isopropyl tris(dodecylbenzene sulfonyl) titanate and bis(dioctyl pyrophosphate) ethylene titanate.
[0043] In the present invention, the molecular weight of the surface modifier is preferably 300 to 3000, more preferably 900 to 1600, and even more preferably 1000 to 1500.
[0044] In the present invention, the mass fraction of the surface modifier is preferably 0.6 to 1.2 parts, more preferably 0.6 to 1 part, and more preferably 0.8 part.
[0045] In the present invention, starch and talc are modified by a chemical surface coating method. A layer of surface modifier is coated on the surface of starch and talc to form a core-shell structure with alkylated starch and alkylated talc as the core and the surface modifier as the shell, which effectively solves the agglomeration problem between starch and talc and increases the compatibility between them and PLA.
[0046] In the present invention, the plasticizer is preferably one or more of plant oil degradable epoxy methyl ester, acetylated castor oil methyl ester, polyglycerol ester, and N,N'-ethylene bisstearamide, further preferably multiple of plant oil degradable epoxy methyl ester, acetylated castor oil methyl ester, and N,N'-ethylene bisstearamide, and more preferably two of plant oil degradable epoxy methyl ester and N,N'-ethylene bisstearamide.
[0047] The present invention does not limit the types of the plant oil-degradable epoxy methyl ester, and the types familiar to those skilled in the art may be used.
[0048] In the present invention, the molecular weight of the polyglycerol ester is preferably 300-750, more preferably 500-750, and even more preferably 700-750.
[0049] In the present invention, the mass fraction of the plasticizer is preferably 0.5 to 9 parts, more preferably 1 to 6 parts, and even more preferably 3 parts.
[0050] In the present invention, the stabilizer is preferably one or more of calcium octadecanoate, zinc octadecanoate, and barium octadecanoate, more preferably one or two of calcium octadecanoate and barium octadecanoate, and more preferably calcium octadecanoate.
[0051] In the present invention, the weight percentage of the stabilizer is preferably 0.5 to 1.8 parts, more preferably 0.5 to 1 part, and more preferably 1 part.
[0052] In the present invention, the antioxidant is preferably tris(2,4-di-tert-butylphenyl)phosphite (antioxidant 168) and / or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (antioxidant 1010), and more preferably a mixture of tris(2,4-di-tert-butylphenyl)phosphite and pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
[0053] In the present invention, the weight percentage of the antioxidant is preferably 0.4 to 0.5 parts, more preferably 0.45 to 0.5 parts, and more preferably 0.5 parts.
[0054] The present invention also provides a method for preparing the special masterbatch for degradable foaming shoe materials, comprising the following steps:
[0055] (1) talcum powder, starch and a surface modifier are mixed and modified to obtain a mixture of modified talcum powder and starch;
[0056] (2) mixing the mixture of modified talcum powder and starch with polylactic acid, and then adding a plasticizer, a stabilizer, and an antioxidant to obtain a mixed material;
[0057] (3) Extruding and granulating the mixed material in turn to obtain a masterbatch for biodegradable foaming shoe material.
[0058] In the present invention, when the temperature of the modification in step (1) is 120≤T≤150°C, the rotation speed of the mixing in step (1) is preferably 300-500 r / min, more preferably 350-430 r / min, and more preferably 400 r / min; when the temperature of the modification in step (1) is 150<T≤170°C, the rotation speed of the mixing in step (1) is preferably 180-260 r / min, more preferably 190-250 r / min, and more preferably 240 r / min;
[0059] The modification time in step (1) is preferably 15 to 25 minutes, more preferably 16 to 24 minutes, and even more preferably 22 minutes.
[0060] In the present invention, the modification in step (1) preferably further includes cooling.
[0061] In the present invention, when the temperature of the mixture of modified talcum powder and starch and polylactic acid in step (2) is 100≤T≤120°C, the mixing speed is preferably 100-200r / min, more preferably 120-180r / min, and more preferably 160r / min; when the temperature of the mixture of modified talcum powder and starch and polylactic acid in step (2) is 80≤T<100°C, the mixing speed is preferably 400-600r / min, more preferably 450-550r / min, and more preferably 500r / min.
[0062] In the present invention, the time for mixing the modified talc powder, starch mixture and polylactic acid in step (2) is preferably 5 to 10 minutes, more preferably 6 to 9 minutes, and even more preferably 8 minutes.
[0063] In the present invention, the rotation speed of the mixing of the plasticizer, stabilizer and antioxidant in step (2) is preferably 300-600 r / min, more preferably 380-500 r / min, more preferably 420 r / min; the temperature is preferably 110-120°C, more preferably 110-115°C, more preferably 110°C; the time is preferably 3-5 min, more preferably 3.5-4.5 min, more preferably 4 min.
[0064] In the present invention, step (2) preferably further comprises cooling after adding the plasticizer, stabilizer and antioxidant and mixing. Specifically in the embodiment of the present invention, the cooling temperature is 90°C.
[0065] In the present invention, steps (1) to (2) are preferably carried out in a high-speed mixer.
[0066] In the present invention, the process parameters of the extrusion granulation in step (3) are preferably: extrusion temperature of 160-180°C, screw speed of 300-500r / min, melt pressure of 7-10MPa, and extrusion current of 70-80% of the rated current;
[0067] Further preferably, the extrusion temperature is 165-175°C, the screw speed is 350-450r / min, the melt pressure is 7-9MPa, and the extrusion current is 70-75% of the rated current;
[0068] More preferably, the extrusion temperature is 170° C., the screw speed is 400 r / min, the melt pressure is 8 MPa, and the extrusion current is 70% of the rated current.
[0069] In the present invention, the pelletizing in step (3) is preferably preceded by cooling by air-cooling.
[0070] In the present invention, the size of the pellets in step (3) is preferably 2 to 3 mm.
[0071] In the present invention, when the degradable foaming shoe material masterbatch is used to prepare disposable slipper soles, no other resin raw materials need to be added. Only an appropriate amount of masterbatch can be added according to the needs and uses.
[0072] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0073] Example 1
[0074] This embodiment provides a method for preparing the degradable foaming shoe material masterbatch, such as Figure 1 As shown, the following steps are included:
[0075] (1) 30 parts of talc (D50: 3.2 μm, silicon content: 42%, whiteness: 92 degrees), 10 parts of corn starch (particle size: 16.3 μm, molecular weight: 8300) and 0.6 parts of isopropyl tri(dodecylbenzenesulfonyl) titanate were placed in a high-speed mixer and stirred at 350 r / min. The heating control device of the high-speed mixer was turned on to control the temperature to 140° C. The mixture was modified for 17 minutes to obtain a mixture of modified talc and starch, which was then cooled.
[0076] (2) 60 parts of PLA (molecular weight 102) were weighed and added to a high-speed mixer, and mixed with the cooled mixture of modified talc and starch at 115° C. and 180 r / min for 8 min. Then, a plasticizer (0.5 parts of vegetable oil degradable epoxy methyl ester (manufacturer Suzhou Huace Environmental Protection Technology Co., Ltd., brand HC-180), 1 part of acetylated castor oil methyl ester, 1 part of N,N'-ethylene bisstearamide, 0.5 parts of polyglycerol ester (molecular weight 750)), a stabilizer (0.5 parts of octadecanoic acid calcium salt, 0.5 parts of octadecanoic acid zinc salt), and an antioxidant (0.2 parts of antioxidant 168 and 0.3 parts of antioxidant 1010) were added to the high-speed mixer, and mixed at 350 r / min for 5 min. After the material temperature reached 110° C., the mixed material was discharged into a water ring sandwich cooler for cooling, and after cooling to 90° C., it was discharged into an extruder silo to obtain a mixed material;
[0077] (3) The mixed material is fed into an extruder for extrusion granulation, the extruder temperature is set to 160° C., the screw speed is 400 r / min, the melt pressure is 7.6 MPa, and the extrusion current is 70% of the rated current; the material is conveyed to a pelletizer for pelletizing by an air-cooled drawing method, and the particle size is maintained at 2 to 3 mm. The prepared particles are conveyed by air to a finished product silo with heating and drying for drying, and the product moisture is maintained at ≤0.1%. The product is packaged to obtain a masterbatch for biodegradable foaming shoe materials.
[0078] Example 2
[0079] This embodiment provides a method for preparing the degradable foaming shoe material masterbatch, comprising the following steps:
[0080] (1) 40 parts of talc (D50 is 4.1 μm, silicon content is 43%, whiteness is 93 degrees), 10 parts of cassava starch (particle size is 17.3 μm, molecular weight is 9000), and 0.8 parts of a mixture of isopropyl tri(dodecylbenzenesulfonyl) titanate and bis(dioctyl pyrophosphate) ethylene titanate (the mass ratio of isopropyl tri(dodecylbenzenesulfonyl) titanate to bis(dioctyl pyrophosphate) ethylene titanate is 1:2) are put into a high-speed mixer, stirred at 400 r / min, and the heating control device of the high-speed stirrer is turned on to control the temperature to 150° C. The mixture is modified for 16 minutes to obtain a mixture of modified talc and starch, and then cooled;
[0081] (2) 55 parts of PLA (molecular weight 105) were weighed and added to a high-speed mixer, and mixed with the cooled mixture of modified talc and starch at 120° C. and 180 r / min for 10 min. Then, a plasticizer (0.5 parts of vegetable oil-degradable epoxy methyl ester (manufacturer Suzhou Huace Environmental Protection Technology Co., Ltd., brand HC-180), 1 part of N,N'-ethylene bisstearamide, 1.5 parts of polyglycerol ester (molecular weight 750)), a stabilizer (0.5 parts of octadecanoic acid calcium salt), and an antioxidant (0.3 parts of antioxidant 168 and 0.2 parts of antioxidant 1010) were added to the high-speed mixer, and mixed at 380 r / min for 4 min. After the material temperature reached 110° C., the mixed material was discharged into a water ring sandwich cooler for cooling, and after cooling to 90° C., it was discharged into the extruder silo to obtain a mixed material;
[0082] (3) The mixed material is fed into an extruder for extrusion granulation, the extruder temperature is set to 170° C., the screw speed is 380 r / min, the melt pressure is 8.5 MPa, and the extrusion current is 76% of the rated current; the material is conveyed to a pelletizer for pelletizing by air-cooled drawing, and the particle size is maintained at 2 to 3 mm. The prepared particles are conveyed by air to a finished product silo with heating and drying for drying, and the product moisture is maintained at ≤0.1%. The product is packaged to obtain a masterbatch for biodegradable foaming shoe materials.
[0083] Example 3
[0084] This embodiment provides a method for preparing the degradable foaming shoe material masterbatch, comprising the following steps:
[0085] (1) 50 parts of talc (D50 is 4.5 μm, silicon content is 44%, whiteness is 93), 10 parts of cassava starch (particle size is 18.4 μm, molecular weight is 8800), and 1 part of a mixture of isopropoxy tri(dioctyl phosphate acyloxy) titanate and isopropyl tri(dodecylbenzene sulfonyl) titanate (the mass ratio of isopropoxy tri(dioctyl phosphate acyloxy) titanate to isopropyl tri(dodecylbenzene sulfonyl) titanate is 2:1) are put into a high-speed mixer, stirred at 430 r / min, and the heating control device of the high-speed stirrer is turned on to control the temperature to 140° C. The mixture is modified for 20 minutes to obtain a mixture of modified talc and starch, and then cooled;
[0086] (2) 60 parts of PLA (molecular weight 105) were weighed and added to a high-speed mixer, and mixed with the cooled mixture of modified talc and starch at 90° C. and 480 r / min for 5 min. Then, a plasticizer (1.5 parts of vegetable oil-degradable epoxy methyl ester (manufacturer Suzhou Huace Environmental Protection Technology Co., Ltd., brand HC-180), 1 part of N,N'-ethylene bisstearamide), a stabilizer (0.5 parts of octadecanoic acid calcium salt, 0.5 parts of octadecanoic acid barium salt), and an antioxidant (0.4 parts of antioxidant 168 and 0.1 parts of antioxidant 1010) were added to the high-speed mixer, and mixed at 470 r / min for 4 min. After the material temperature reached 110° C., the mixed material was discharged into a water ring sandwich cooler for cooling, and after cooling to 90° C., it was discharged into the extruder silo to obtain a mixed material;
[0087] (3) The mixed material is put into an extruder for extrusion granulation, the extruder temperature is set to 170° C., the screw speed is 450 r / min, the melt pressure is 9.2 MPa, and the extrusion current is 76% of the rated current; the material is conveyed to a pelletizer for pelletizing by air-cooled drawing, and the particle size is maintained at 2 to 3 mm. The prepared particles are conveyed by air to a finished product silo with heating and drying for drying, and the product moisture is maintained at ≤0.1%. The product is packaged to obtain a masterbatch for biodegradable foaming shoe materials.
[0088] Comparative Example 1
[0089] (1) 60 parts of cassava starch (particle size 17.3 μm, molecular weight 9000), 1 part of a mixture of isopropoxy tri(dioctyl phosphate acyloxy) titanate and isopropyl tri(dodecylbenzene sulfonyl) titanate (the mass ratio of isopropoxy tri(dioctyl phosphate acyloxy) titanate to isopropyl tri(dodecylbenzene sulfonyl) titanate is 2:1) are put into a high-speed mixer, stirred at 450 r / min, the heating control device of the high-speed stirrer is turned on, the temperature is controlled to 130° C., the modification is carried out for 19 minutes to obtain the modified starch, and the mixture is cooled;
[0090] (2) 60 parts of PLA (molecular weight 104) were weighed and added to a high-speed mixer, and mixed with the cooled modified starch at 100° C. and 460 r / min for 8 min. Then, a plasticizer (1.5 parts of vegetable oil-degradable epoxy methyl ester (manufacturer Suzhou Huace Environmental Protection Technology Co., Ltd., brand HC-180), 1 part of N,N'-ethylene bisstearamide), a stabilizer (0.5 parts of calcium octadecanoate, 0.5 parts of barium octadecanoate), and an antioxidant (0.1 parts of antioxidant 168 and 0.4 parts of antioxidant 1010) were added to the high-speed mixer, and mixed at 480 r / min for 3 min. After the material temperature reached 110° C., the mixed material was discharged into a water ring sandwich cooler for cooling, and after cooling to 90° C., it was discharged into the extruder silo to obtain a mixed material;
[0091] (3) The mixed material is fed into an extruder for extrusion granulation, the extruder temperature is set to 175° C., the screw speed is 460 r / min, the melt pressure is 8.9 MPa, and the extrusion current is 74% of the rated current; the material is conveyed to a pelletizer for pelletizing by air-cooled drawing, and the particle size is maintained at 2 to 3 mm. The prepared particles are conveyed by air to a finished product silo with heating and drying for drying, and the product moisture is maintained at ≤0.1%. The product is packaged to obtain a masterbatch for biodegradable foaming shoe materials.
[0092] Experimental example
[0093] The masterbatches prepared in Examples 1 to 3 and Comparative Example 1 were heated in an oven at 105°C for 10 min to control the moisture content of the masterbatches below 0.05%. The dehumidified and dried raw materials were added to the extruder for internal mixing - open mixing - shaping of the sheet - slicing - foaming - product. The internal mixing temperature was 160°C, the open mixing temperature was 200°C, and the roller speed was 30r / min to prepare 120g / m 2 Thickness of foam sheet.
[0094] The density of the foaming masterbatch was tested according to GB 1033-86 “Test method for density and relative density of plastics”, the foaming ratio was calculated by the volume ratio of the same mass of foaming material and plastic masterbatch, and the melt strength was tested using a melt strength tester. The results are shown in Table 1.
[0095] Table 1. Test results of foamed sheet properties of masterbatches obtained in Examples 1 to 3 and Comparative Example 1
[0096] sample <![CDATA[Density of foaming masterbatch (g / cm 3 )]]> Foaming ratio Melt strength (N) Example 1 1.31 18 26 Example 2 1.23 19 24 Example 3 1.25 17 27 Comparative Example 1 1.51 12 14
[0097] It can be seen from Table 1 that the density of the degradable masterbatch in the embodiment is lower than that in the comparative example, and the foaming ratio and melt strength are higher, in which only starch is added as a filler.
[0098] The degradable plastic masterbatches of Examples 1 to 3 and Comparative Example 1 were injection molded into thin plastic samples of 1 cm×1 cm×1 cm, dried to constant weight and buried in the soil at a depth of about 20 cm in a natural environment. The samples were taken out after 60 days, rinsed and dried to constant weight, and the degradation mass loss rate of each group was calculated.
[0099] Table 2. Degradation mass loss rate
[0100] sample Degradation mass loss rate Example 1 80% Example 2 81% Example 3 82% Comparative Example 1 86%
[0101] It can be seen from Table 2 that the foamed plastic masterbatch of the present invention has good biodegradability, is environmentally friendly, and helps to reduce the "white pollution" caused by discarded products.
[0102] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A masterbatch for degradable foaming shoe materials, characterized in that: Contains the following raw materials in parts by weight: 40-70 parts of polylactic acid, 10-20 parts of starch, 30-50 parts of talc, 0.4-1.4 parts of surface modifier, 0.16-11.2 parts of plasticizer, 0.5-2.8 parts of stabilizer, 0.3-0.5 parts of antioxidant; The surface modifier is one or more of isopropoxy tris(dioctyl phosphate) titanate, isopropyl tris(dodecylbenzenesulfonyl) titanate and bis(dioctyl pyrophosphate) ethylene titanate.
2. The special masterbatch for degradable foaming shoe material according to claim 1, characterized in that: The starch is one or more of corn starch, potato starch and cassava starch, and the average particle size of the starch is 15 to 20 μm.
3. A masterbatch for degradable foaming shoe materials as claimed in claim 1 or 2, characterized in that: The specifications of the talcum powder are: D50 is 3-5 μm, silicon content is 40-45%, and whiteness is 91-94 degrees.
4. The special masterbatch for degradable foaming shoe material according to claim 1, characterized in that: The plasticizer is one or more of plant oil degradable epoxy methyl ester, acetylated castor oil methyl ester, polyglycerol ester, N,N'-ethylene bisstearamide; the stabilizer is one or more of octadecanoic acid calcium salt, octadecanoic acid zinc salt, and octadecanoic acid barium salt.
5. A masterbatch for degradable foaming shoe materials as claimed in claim 1 or 4, characterized in that: The antioxidant is tris(2,4-di-tert-butylphenyl)phosphite and / or pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate].
6. The method for preparing a masterbatch for degradable foaming shoe materials according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) talcum powder, starch and a surface modifier are mixed and modified to obtain a mixture of modified talcum powder and starch; (2) mixing the mixture of modified talcum powder and starch with polylactic acid, and then adding a plasticizer, a stabilizer, and an antioxidant to obtain a mixed material; (3) Extruding and granulating the mixture in turn to obtain a masterbatch for biodegradable foaming shoe materials.
7. The method for preparing a special masterbatch for degradable foaming shoe materials according to claim 6, characterized in that: When the temperature of the modification in step (1) is 120≤T≤150°C, the rotation speed of the mixing in step (1) is 300-500 r / min; when the temperature of the modification in step (1) is 150<T≤170°C, the rotation speed of the mixing in step (1) is 180-260 r / min; The modification time in step (1) is 15 to 25 minutes.
8. The method for preparing a special masterbatch for degradable foaming shoe materials according to claim 6, characterized in that: When the temperature of the mixture of modified talcum powder and starch and polylactic acid in step (2) is 100≤T≤120°C, the mixing speed is 100-200r / min; when the temperature of the mixture of modified talcum powder and starch and polylactic acid in step (2) is 80≤T<100°C, the mixing speed is 400-600r / min; In step (2), the time for mixing the modified talcum powder, starch mixture and polylactic acid is 5 to 10 minutes.
9. The method for preparing a special masterbatch for degradable foaming shoe materials according to claim 6 or 8, characterized in that: The mixing speed of adding the plasticizer, stabilizer and antioxidant in step (2) is 300-600 r / min, the temperature is 110-120° C., and the time is 3-5 min.
10. The method for preparing a special masterbatch for degradable foaming shoe materials according to claim 6 or 7, characterized in that: The process parameters of the extrusion granulation in step (3) are: extrusion temperature of 160-180° C., screw speed of 300-500 r / min, melt pressure of 7-10 MPa, and extrusion current of 70-80% of the rated current.