Self-lubricating polyurethane composite material as well as preparation method and application thereof
By adding phase change materials to the polyurethane material to form a lubricating film, the problems of heat absorption and lubrication of polyurethane materials during friction are solved, the tribological performance and service life are improved, and it is suitable for a variety of working conditions.
Patent Information
- Application Number
- CN202411104160.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
During the friction process, existing polyurethane materials have problems with solid lubricating materials that are difficult to disperse and liquid lubricating materials that are easy to leak, resulting in reduced mechanical properties and service life.
The composite of phase change material and polyurethane prepolymer is adopted to absorb heat during the friction process through the phase change material, form a lubricating film, reduce the friction coefficient and improve wear resistance, and form a stable composite material through cross-linking of curing agent.
It improves the tribological properties of polyurethane composites in dry friction, pure water and seawater environments, extends service life, reduces friction coefficient and wear rate, and is suitable for a variety of working conditions, especially for high-load applications.
Smart Images

Figure CN118931166A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a self-lubricating polyurethane composite material and a preparation method and application thereof. Background Art
[0002] Polyurethane materials are a type of material that has both rubber and plastic properties, and have excellent tensile strength, tear strength, wear resistance, impact resistance, weather resistance, hydrolysis resistance, and oil resistance. They are widely used in elastomers, foam materials, coatings, adhesives, and biomedical materials. Self-lubricating polyurethane is a special polymer material. By adding lubricating materials or modifying the surface of polyurethane materials, a lower friction coefficient and excellent wear resistance can be obtained. This material has wide application potential in the engineering field. The current method to reduce the friction coefficient of polyurethane materials and improve self-lubrication is mainly to add lubricating materials during the polyurethane synthesis process to reduce the friction and wear of polyurethane materials. Traditional lubricating materials mainly include solid lubricating materials and liquid lubricating materials. Solid lubricating materials include fillers such as molybdenum disulfide, graphite, talcum powder and boron nitride. These solid lubricating materials have good friction reduction and wear resistance effects, but solid lubricating materials and polyurethane matrix have the problem of difficult dispersion, and their mechanical properties are difficult to achieve the effect of material design; liquid lubricating materials mainly include plant lubricants, animal lubricants, mechanical oils and silicone oils. These materials need to consider the leakage of liquid lubricating materials and the requirements of the preparation process during use. At the same time, polyurethane materials generate dynamic mechanical losses and friction within the molecular chain during the friction process, which gradually increases the endogenous heat of the material. The generation of this endogenous heat has an impact on the product performance and service life of the material. Therefore, the design of new self-lubricating polyurethane materials has become an urgent need to solve the growing demand for high performance of polyurethane materials in the current industrial field, and has important guiding significance. Summary of the invention
[0003] In order to improve the problems that solid lubricating materials are difficult to disperse in a polyurethane matrix, liquid lubricating materials are easy to leak, and polyurethane generates internal heat under friction, resulting in reduced mechanical properties and service life, and in order to improve the friction-reducing and wear-resistant properties of polyurethane elastomers, the present invention provides a self-lubricating polyurethane composite material, a preparation method and application thereof.
[0004] The present invention provides a self-lubricating polyurethane composite material, which adopts the following technical solution: A self-lubricating polyurethane composite material comprises, by weight, 90-110 parts of polyurethane prepolymer, 0.1-50 parts of phase change material, 20-50 parts of curing agent, and 0.1-1 part of defoaming agent.
[0005] Furthermore, the alkane phase change material or the fatty acid phase change material is any one or a mixture of any two.
[0006] Furthermore, the alkane phase change material includes any one or more of n-octadecane, n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane and n-triacontane.
[0007] Furthermore, the fatty acid phase change material includes any one or more of lauric acid, palmitic acid and stearic acid.
[0008] Furthermore, the polyurethane prepolymer is prepared by reacting polyol and isocyanate.
[0009] Furthermore, the polyol includes any one of polytetramethylene carbonate diol and polyhexamethylene carbonate diol; the isocyanate includes any one of hexamethylene diisocyanate, toluene diisocyanate, triphenylmethane triisocyanate, 1,5-naphthalene diisocyanate and isophorone diisocyanate or a mixture of any two thereof; and the isocyanate group (-NCO) content in the polyurethane prepolymer is 6-35%.
[0010] Further, the curing agent includes any one of 4,4′-methylenebis(2-chloroaniline), 4,4′-methylenebis(3-chloro-2,6-diethylaniline), methylenebis-o-chloroaniline, 4,4′-methylene-bis-(2,6-diethylaniline) and 4,4′-di-sec-butylaminodiphenylmethane.
[0011] Furthermore, the defoaming agent includes any one of YRXP-07B, YRXP-07A, YRXP-06 and BYK-066N.
[0012] The present invention provides a method for preparing a self-lubricating polyurethane composite material, comprising the following steps: Step 1: Mix the polyurethane prepolymer with the phase change material, and perform vacuum degassing at a temperature above the phase change temperature of the phase change material. Specifically, perform vacuum degassing at 70-85° C. for 2-6 hours. Step 2: then adding a curing agent and a defoaming agent, stirring at a stirring speed of 20 to 10,000 r / min for 10 to 60 seconds to obtain a uniform mixed solution, vacuuming the mixed solution to remove bubbles, and maintaining the temperature of the mixed solution above the phase change temperature of the phase change material; Step 3: Pour the mixed solution into a preheated mold, heat the mold to the reaction temperature of the curing agent, and crosslink and cure the polymer. Specifically, the mold temperature is controlled at 90-110°C and cured for 2-48 hours. After the reaction is complete, a self-lubricating polyurethane composite material is obtained.
[0013] The present invention also provides the use of the self-lubricating polyurethane composite material in friction pair components such as water-lubricated bearings, bridge liners, sliders and guide rails in the field of mechanical engineering equipment such as ships, cross-sea bridges, drilling platforms and deep-sea exploration.
[0014] The friction reduction and wear resistance principle of the present invention is as follows: phase change material is a type of material whose temperature change value tends to zero when phase change occurs, but can absorb or release a large amount of heat. Since this type of material has a small volume change and a large latent heat when phase change occurs, it absorbs the heat generated by the polyurethane composite material during the friction process, and will not cause the polyurethane composite material to fail due to excessive temperature increase. When the polyurethane composite material contains a phase change material, the heat generated during the friction process is transferred to the phase change material, and the phase change material absorbs the heat and undergoes a phase change, preventing the surface temperature of the polyurethane composite material from rising rapidly, thereby preventing the polymer material from thermally degrading due to excessively high temperature, and preventing the mechanical properties of the material from failing. Therefore, through the phase change of the phase change material, the polyurethane composite material can be guaranteed to work within a suitable temperature range.
[0015] The polyurethane material and the phase change material melt into liquid above the phase change temperature of the phase change material, and after being stirred evenly, they are cross-linked and solidified into one under the action of a curing agent. Under the action of frictional heat, stress and other forces, the phase change material will be released from the polyurethane composite material, thereby forming a lubricating film at the friction interface, which works together with the water film formed on the surface of the polyurethane material in the water environment to reduce the friction coefficient and improve the wear resistance. At the same time, as a material for water-lubricated bearings, the polyurethane composite material can have a longer service life due to water lubrication and water thermal conductivity. At the same time, because the polyurethane composite material can form a lubricating film under dry friction conditions, it can solve the problem of water-lubricated bearings being prone to ablation during dry friction startup.
[0016] In summary, the present invention includes at least one of the following beneficial technical effects: 1. By compounding phase change materials and polyurethane materials, the tribological properties of polyurethane composite materials in dry friction, pure water and seawater environments can be improved, and they can have broad application prospects under various working conditions; alkane phase change materials and fatty acid phase change materials are low in cost, have a wide phase change temperature range and have excellent tribological properties.
[0017] 2. The self-lubricating polyurethane composite material of the present invention has broad application prospects in the fields of mechanical engineering equipment such as ships, cross-sea bridges, offshore drilling platforms and deep-sea exploration as friction pair components such as water-lubricated bearings, bridge support slides, sliders and guide rails. The main structure of polyurethane and phase change material is adopted, so that it has excellent self-lubricating characteristics and friction reduction and wear resistance. In addition, the preparation conditions of the self-lubricating polyurethane composite material of the present invention are mild, the preparation process has good repeatability, low preparation cost, simple operation and is suitable for large-scale production.
[0018] 3. The self-lubricating polyurethane composite material prepared by the present invention also has the following advantages: (1) Low friction coefficient: This material is able to form a lubricating film between the friction surfaces of the materials, thereby reducing energy consumption and wear.
[0019] (2) Good self-lubricating properties: Through compounding with phase change materials, self-lubricating polyurethane materials exhibit excellent self-lubricating properties, which are especially suitable for high-load applications. Phase change materials also have a friction-reducing effect in a solid state, entering the interface to protect the polyurethane matrix and bearings.
[0020] (3) Low wear rate: Compared with traditional polyurethane materials, self-lubricating polyurethane composites have a lower wear rate, giving the material a longer service life.
[0021] (4) Improved thermal conductivity: The self-lubricating polyurethane composite material contains phase change material, which keeps the material's operating temperature stable during the friction process, so the material has better thermal stability. (5) Mechanical properties: Self-lubricating polyurethane materials have high tensile strength and elongation at break, enabling them to withstand large loads.
[0022] (6) Environmentally friendly: During the production process, the self-lubricating polyurethane composite material does not contain harmful volatiles, and the preparation process is simple to operate, which can reduce the impact on the environment and employee health.
[0023] (7) Wide application potential: Due to its excellent comprehensive performance, self-lubricating polyurethane composites can be used in a variety of engineering fields, such as machinery industry, shipbuilding industry, building materials, transportation, etc. BRIEF DESCRIPTION OF THE DRAWINGS Figure 1 The differential scanning calorimeter (DSC) curves of the polyurethane materials prepared in Example 1 and Comparative Example 1 of the present invention are shown.
[0024] Figure 2 This is a scanning electron microscope (SEM) image of the cross section of the self-lubricating polyurethane composite material prepared in Example 1 of the present invention (the scale is 100 microns).
[0025] Figure 3 This is a scanning electron microscope (SEM) image of the cross section of the self-lubricating polyurethane composite material prepared in Example 1 of the present invention (the scale is 50 microns).
[0026] Figure 4 1 is a relationship diagram between the friction coefficient and the friction time of Example 1, Example 10 and Comparative Example 1 of the present invention under dry friction conditions (load is 50 N, rotation speed is 500 r / min).
[0027] Figure 5The wear volume diagrams of Example 1, Example 10 and Comparative Example 1 of the present invention under dry friction conditions (load is 50 N, rotation speed is 500 r / min).
[0028] Figure 6 1 is a relationship diagram between the friction coefficient and the friction time of Example 1, Example 10 and Comparative Example 1 of the present invention under pure water conditions (load is 50 N, rotation speed is 500 r / min).
[0029] Figure 7 The wear volume diagram of Example 1, Example 10 and Comparative Example 1 of the present invention under pure water conditions (load is 50N, rotation speed is 500 r / min).
[0030] Figure 8 1 is a relationship diagram between the friction coefficient and the friction time of Example 1, Example 10 and Comparative Example 1 of the present invention under seawater conditions (load is 50 N, rotation speed is 500 r / min).
[0031] Fig. 9 The wear volume diagram of Example 1, Example 10 and Comparative Example 1 of the present invention under seawater conditions (load is 50N, rotation speed is 500 r / min). DETAILED DESCRIPTION
[0032] The following embodiments of the present invention are described in further detail in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0033] The preferred embodiments of the present invention will be described in more detail below. Although the following content describes the preferred embodiments of the present invention, it should be understood that the present invention can be implemented with various basic formulations and should not be limited by the formulations used herein. On the contrary, these formulations are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0034] Comparative Example 1: 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 9%) was vacuum degassed at 75 °C for 3 hours, and then 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N were added and stirred at 1000 r / min for 60 seconds. After vacuum removal of bubbles, the mixed solution was poured into a preheated mold, the mold temperature was controlled at 100 °C, and the curing time was 24 hours to obtain a polyurethane composite material.
[0035] Example 1 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 9%) is mixed with 20 kg of n-hexacosane, and vacuum degassing is carried out at 75 °C for 3 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 1000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0036] The DSC curve of the self-lubricating polyurethane composite material is shown in Figure 1 As shown in the figure, it can be found that the self-lubricating polyurethane material prepared in Example 1 has a melting peak (58.1 °C), the phase change material has a melting peak (56.8 °C), and the polyurethane material prepared in Comparative Example 1 has no melting peak, indicating that the prepared self-lubricating polyurethane composite material contains a phase change material and has phase change properties.
[0037] pass Figure 2 and Figure 3 From the SEM cross-sectional view, it can be seen that the spherical particles of the phase change material are evenly distributed in the polyurethane matrix, where the diameter of the phase change material particles is 10-40 μm. At the same time, there is a gap between the phase change material and the matrix, indicating that the interfacial bonding force between the phase change material and the polyurethane matrix is weak. The above reason is that the phase change material is a non-polar substance, while polyurethane is a polar substance. During the preparation process, the "water-in-oil" phenomenon occurs through stirring, thereby forming spherical particles. When friction occurs, the phase change material forms a lubricating film on the friction interface due to the influence of friction heat, thereby improving the tribological properties of the polyurethane composite material and achieving the effect of reducing friction and resisting wear.
[0038] Example 2 110 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 35%) is mixed with 0.1 kg of n-octadecane, and vacuum degassing is carried out at 70 °C for 2 hours. Then, 10 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 20 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 2 hours. The obtained material is a self-lubricating polyurethane composite material.
[0039] Example 3 90 kg of polyurethane prepolymer (polyol is polyhexamethylene carbonate diol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 6%) is mixed with 50 kg of n-docosane, and vacuum degassing is carried out at 85 °C for 6 hours. Then, 50 kg of 4,4′-methylenebis(2-chloroaniline) and 1 kg of BYK-066N are added and stirred at 10000 r / min for 10 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 48 hours. The obtained material is a self-lubricating polyurethane composite material.
[0040] Example 4 100 kg of polyurethane prepolymer (polyol is polyhexamethylene carbonate diol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 10%) is mixed with 20 kg of n-tetracosane, and vacuum degassing is carried out at 75 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.5 kg of BYK-066N are added and stirred at 1000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 12 hours. The obtained material is a self-lubricating polyurethane composite material.
[0041] Example 5 95 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 13%) is mixed with 15 kg of n-eicosane and 15 g of n-octadecane, and vacuum degassing is carried out at 75 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.5 kg of BYK-066N are added and stirred at 1000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 40 hours. The obtained material is a self-lubricating polyurethane composite material.
[0042] Example 6 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 13%) is mixed with 15 kg of n-octacosane, and vacuum degassing is carried out at 75 °C for 6 hours. Then, 35 kg of 4,4′-methylenebis(2-chloroaniline) and 0.3 kg of BYK-066N are added and stirred at 2500 r / min for 45 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 36 hours. The obtained material is a self-lubricating polyurethane composite material.
[0043] Example 7 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 15%) is mixed with 20 kg of n-triacontane, and vacuum degassing is carried out at 72 °C for 6 hours. Then, 30 kg of 4,4′-methylenebis(2-chloroaniline) and 0.2 kg of BYK-066N are added and stirred at 500 r / min for 30 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0044] Example 8 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 15%) is mixed with 40 kg of n-octacosane, and vacuum degassing is carried out at 72 °C for 6 hours. Then, 30 kg of 4,4′-methylenebis(2-chloroaniline) and 0.2 kg of BYK-066N are added and stirred at 5000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0045] Example 9 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 10%) is mixed with 10 kg of n-octacosane, and vacuum degassing is carried out at 72 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 2000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0046] Example 10 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 9%) is mixed with 5 kg of n-octacosane, and vacuum degassing is carried out at 72 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 2000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0047] Embodiment 11 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 9%) is mixed with 2.5 kg of n-hexacosane, and vacuum degassing is carried out at 70 °C for 4 hours. Then, 27 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 3000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0048] Example 12 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 20%) is mixed with 20 kg of n-hexacosane, and vacuum degassing is carried out at 75 °C for 4 hours. Then, 27 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 3000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 36 hours. The obtained material is a self-lubricating polyurethane composite material.
[0049] Example 13 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 9.5%) is mixed with 20 kg of n-octacosane, and vacuum degassing is carried out at 75 °C for 4 hours. Then, 30 kg of 4,4′-methylenebis(2-chloroaniline) and 0.1 kg of BYK-066N are added and stirred at 3000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0050] Embodiment 14 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 10%) is mixed with 10 kg of lauric acid, and vacuum degassing is carried out at 72 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(3-chloro-2,6-diethylaniline) and 0.1 kg of BYK-066N are added and stirred at 2000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 110 °C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0051] Embodiment 15 100 kg of polyurethane prepolymer (polyol is polytetramethylene diol, isocyanate is hexamethylene diisocyanate, and the -NCO content of the prepolymer is 10%) is mixed with 5 kg of lauric acid and 5 kg of palmitic acid, and vacuum degassing is carried out at 75 °C for 5 hours. Then, 29 kg of methylene dichloroaniline and 0.2 kg of BYK-066N are added and stirred at 2500 r / min for 60 seconds. After vacuum removal of bubbles, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 90 °C, and the curing time is 25 hours. The obtained material is a self-lubricating polyurethane composite material.
[0052] Example 16 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is toluene diisocyanate, and the -NCO content of the prepolymer is 20%) is mixed with 5 kg of lauric acid and 10 kg of stearic acid, and vacuum degassing is carried out at 72 ° C for 6 hours, and then 35 kg of 4,4′-methylene-bis-(2,6-diethylaniline) and 0.1 kg of BYK-066N are added and stirred at 2000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 ° C, and the curing time is 24 hours. The obtained material is a self-lubricating polyurethane composite material.
[0053] Embodiment 17 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is triphenylmethane triisocyanate, and the -NCO content of the prepolymer is 12%) is mixed with 10 kg of palmitic acid and 10 kg of stearic acid, and vacuum degassing is carried out at 72 °C for 6 hours. Then, 30 kg of 4,4′-di-sec-butylaminodiphenylmethane and 0.3 kg of YRXP-07B are added and stirred at 3000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 36 hours. The obtained material is a self-lubricating polyurethane composite material.
[0054] Embodiment 18 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is 1,5-naphthalene diisocyanate, and the -NCO content of the prepolymer is 10%) is mixed with 20 kg of palmitic acid, and vacuum degassing is carried out at 75 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.5 kg of YRXP-07A are added and stirred at 1000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 95 °C, and the curing time is 12 hours. The obtained material is a self-lubricating polyurethane composite material.
[0055] Embodiment 19 100 kg of polyurethane prepolymer (polyol is polytetramethylene glycol, isocyanate is isophorone diisocyanate, and the -NCO content of the prepolymer is 13%) is mixed with 15 kg of stearic acid, and vacuum degassing is carried out at 75 °C for 6 hours. Then, 28 kg of 4,4′-methylenebis(2-chloroaniline) and 0.5 kg of YRXP-06 are added and stirred at 1000 r / min for 60 seconds. After vacuum degassing, the mixed solution is poured into a preheated mold, the mold temperature is controlled at 100 °C, and the curing time is 40 hours. The obtained material is a self-lubricating polyurethane composite material.
[0056] The tribological properties of the polyurethane composite material samples prepared in the above comparative example 1 and examples 1 and 10 were compared, and the results were as follows: Figure 4-9 .
[0057] Tribological performance test: The SST-ST ball-disc friction and wear tester was used to perform tribological tests on the polyurethane composite material under dry friction, pure water, and artificial seawater lubrication conditions. The moving pair was a ball with a diameter of 7.9375 mm made of GCr15 bearing steel, with a load of 50 N, a speed of 500 r / min, a rotation radius of 21 mm, and a working time of 60 minutes. After the friction experiment, the three-dimensional surface morphology of the wear mark was characterized using a white light copolymerization three-dimensional topography instrument, the width and depth of the wear mark were analyzed, and the wear volume was calculated.
[0058] like Figure 4-9As shown, it can be seen that the pure polyurethane sample of comparative example 1 is compared with the polyurethane composite sample of embodiment 1. Under dry friction, pure water and seawater conditions, the friction coefficient of the polyurethane composite material decreases significantly, and the wear volume also decreases significantly. Especially under dry friction conditions, the pure polyurethane sample of comparative example 1 has a huge wear volume when the friction test is carried out for 300 seconds, which makes it impossible to carry out the test. The friction coefficient of the self-lubricating polyurethane composite material of embodiment 1 is 0.06, and its wear volume is much smaller than the self-made pure polyurethane sample of comparative example 1. The reason is that the polyurethane composite material of embodiment 1 contains phase change material. Since the phase change material can reduce the temperature of the friction interface and produce a lubricating film on the friction interface, it has excellent dry friction performance. The self-lubricating polyurethane composite material prepared by the present invention has excellent friction reduction and anti-wear performance under dry friction, pure water and seawater conditions. The self-lubricating polyurethane composite material has a wide range of application prospects in the fields of mechanical engineering equipment such as ships, cross-sea bridges, drilling platforms and deep-sea exploration as friction pair components such as water-lubricated bearings, bridge support slides, sliders and guide rails.
[0059] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A self-lubricating polyurethane composite material, characterized in that: Calculated by weight, the self-lubricating polyurethane composite material includes 90-110 parts of polyurethane prepolymer, 0.1-50 parts of phase change material, 20-50 parts of curing agent, and 0.1-1 part of defoaming agent.
2. A self-lubricating polyurethane composite material according to claim 1, characterized in that: The phase change material includes any one of an alkane phase change material and a fatty acid phase change material, or a mixture of any two of them.
3. A self-lubricating polyurethane composite material according to claim 2, characterized in that: The alkane phase change material includes any one or more of n-octadecane, n-eicosane, n-docosane, n-tetracosane, n-hexacosane, n-octacosane and n-triacontane.
4. The self-lubricating polyurethane composite material according to claim 2, characterized in that: The fatty acid phase change material includes any one or more of lauric acid, palmitic acid and stearic acid.
5. The self-lubricating polyurethane composite material according to claim 1, characterized in that: The polyurethane prepolymer is prepared by reacting polyol and isocyanate.
6. The self-lubricating polyurethane composite material according to claim 5, characterized in that: The polyol includes any one of polytetramethylene diol and polyhexamethylene carbonate diol; the isocyanate includes any one of hexamethylene diisocyanate, toluene diisocyanate, triphenylmethane triisocyanate, 1,5-naphthalene diisocyanate and isophorone diisocyanate or a mixture of any two thereof; and the isocyanate group content in the polyurethane prepolymer is 6-35%.
7. The self-lubricating polyurethane composite material according to claim 1, characterized in that: The curing agent includes any one of 4,4′-methylenebis(2-chloroaniline), 4,4′-methylenebis(3-chloro-2,6-diethylaniline), methylenebis-o-chloroaniline, 4,4′-methylene-bis-(2,6-diethylaniline) and 4,4′-di-sec-butylaminodiphenylmethane.
8. The self-lubricating polyurethane composite material according to claim 1, characterized in that: The defoaming agent includes any one of YRXP-07B, YRXP-07A, YRXP-06 and BYK-066N.
9. The method for preparing the self-lubricating polyurethane composite material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step 1: Mix the polyurethane prepolymer with the phase change material, and perform vacuum degassing above the phase change temperature of the phase change material; Step 2: Then add the curing agent and the defoaming agent, stir evenly to obtain a uniform mixed solution, remove bubbles from the mixed solution by vacuum, and maintain the temperature of the mixed solution above the phase change temperature of the phase change material; Step 3: Pour the mixed solution into a preheated mold, heat the mold to the reaction temperature of the curing agent, crosslink and cure the polymer, and obtain a self-lubricating polyurethane composite material after the reaction is complete.
10. Application of the self-lubricating polyurethane composite material according to any one of claims 1 to 8 in the fields of water-lubricated bearings, bridge bearing slides, sliders and guide rails.
Citation Information
Cited By
Antifriction and wear-resistant polyamide-imide composite material as well as preparation method and application thereof
CN119931490A
High-performance polyurethane-based water lubricating material and preparation method thereof
CN121271218A