Radiation-resistant low-friction composite film as well as preparation method and application thereof

By introducing zinc and tungsten carbide into the molybdenum disulfide film, the titanium/zinc/molybdenum disulfide/tungsten carbide gradient transition layer and zinc/molybdenum disulfide/tungsten carbide layer are solved, and the traditional molybdenum disulfide film is solved in atomic oxygen radiation. The problem of oxidation has achieved efficient anti-oxidation and low friction performance, meeting the long-term service needs of space devices.

CN118932280APending Publication Date: 2024-11-12NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411112354.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional molybdenum disulfide films are easily oxidized under atomic oxygen radiation, resulting in their mass decline and failure, and cannot meet the long-term service needs of space devices in extreme environments.

Method used

Magneto-controlled sputtering technology is used to deposit titanium transition layer, titanium/zinc/molybdenum disulfide/tungsten carbide gradient transition layer and zinc/molybdenum disulfide/tungsten carbide layer in sequence on the substrate surface to form a composite film that is resistant to radiation and low friction. The synergistic action of zinc and tungsten carbide improves the oxidation resistance and tribological properties of the film.

Benefits of technology

It significantly improves the substrate bond strength, mechanical properties and tribological properties of the film, can maintain good lubricating performance under atomic oxygen radiation, is suitable for the low friction and stable service requirements of aerospace devices, and the preparation method is green, economical and controllable. , suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932280A_ABST
    Figure CN118932280A_ABST
Patent Text Reader

Abstract

The invention discloses an irradiation-resistant low-friction composite film as well as a preparation method and application thereof. The composite film comprises a titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer which are sequentially formed on the surface of a substrate. Wherein in the direction gradually away from the substrate, the content of titanium in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer is gradually reduced, the content of zinc is gradually increased, the content of molybdenum disulfide is gradually increased, and the content of tungsten carbide is gradually increased. The composite film has excellent irradiation resistance and tribological performance, the vacuum friction coefficient of the film is far lower than 0.01 under the atomic oxygen irradiation dose of 6.12 * 10 < 21 > atoms * cm <-2 >, the service requirement of a spacecraft in a near-earth orbit atomic oxygen environment can be met, and scientific basis and theoretical support are provided for the preparation process of the molybdenum disulfide-based film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface lubricating film materials, and in particular relates to a radiation-resistant low-friction composite film and a preparation method and application thereof. Background Art

[0002] The moving parts of spacecraft are in extreme environments rich in atomic oxygen for a long time, so it is necessary to design a molybdenum disulfide film with excellent lubrication properties under atomic oxygen irradiation to extend the service life of the moving parts. Traditional molybdenum disulfide films are prone to oxidation under atomic oxygen irradiation, which affects the quality of the film in advance and even causes failure. Therefore, providing high radiation resistance of the film and reducing the tribological properties of the film are urgent issues to be solved. Summary of the invention

[0003] The main purpose of the present invention is to provide a radiation-resistant, low-friction composite film and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.

[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0005] The embodiment of the present invention provides a radiation-resistant and low-friction composite film, which includes: a titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer sequentially formed on the surface of a substrate;

[0006] Among them, in the direction gradually away from the substrate, the titanium content in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer gradually decreases, the zinc content gradually increases, the molybdenum disulfide content gradually increases, and the tungsten carbide content gradually increases; at the same time, in the direction gradually away from the substrate, zinc, molybdenum disulfide, and tungsten carbide are evenly distributed in the zinc / molybdenum disulfide / tungsten carbide layer.

[0007] An embodiment of the present invention also provides a method for preparing the aforementioned radiation-resistant, low-friction composite film, which comprises: using magnetron sputtering technology to sequentially deposit a titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer on the surface of a substrate, thereby obtaining a radiation-resistant, low-friction composite film.

[0008] The embodiment of the present invention also provides the use of the aforementioned radiation-resistant and low-friction composite film in the field of surface protection of aerospace devices.

[0009] Compared with the prior art, the present invention has the following beneficial effects:

[0010] (1) The radiation-resistant, low-friction composite film provided by the present invention has good substrate bonding strength and mechanical properties, and effectively improves the tribological properties of the film, and can meet the service requirements of low friction and stable lubrication of aerospace devices;

[0011] (2) The radiation-resistant and low-friction composite film provided by the present invention still has good friction and wear performance under atomic oxygen irradiation and has good environmental adaptability;

[0012] (3) The preparation method provided by the present invention is green, economical, controllable, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0014] Figure 1 is a surface SEM image of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention;

[0015] Figure 2 is a cross-sectional SEM image of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention;

[0016] Figure 3 is a cross-sectional TEM image of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention;

[0017] Figure 4 is a graph of hardness and elastic modulus of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention;

[0018] Figure 5 is a friction coefficient diagram of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention;

[0019] Figure 6 is a wear rate diagram of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention;

[0020] Figure 7 This is a friction life diagram of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0021] So far, a lot of research has been done on molybdenum disulfide at home and abroad. Due to the large differences in the performance of films prepared by different processes, vacuum magnetron sputtering technology is a method in which the target material is deposited on the surface of the substrate material under the bombardment of high-energy particles. The surface of the film is denser, the friction performance is excellent, and it is conducive to low-carbon environmental protection. However, its friction reduction mechanism is essentially the shear slip between the transfer film and the long-range structure of the wear scar surface, making it difficult to achieve sustained and stable ultra-low friction and wear and good oxidation resistance.

[0022] In view of the defects of the prior art, the inventors of this case, after long-term research and extensive practice, were able to propose the technical solution of the present invention, which mainly uses magnetron sputtering technology to introduce zinc and tungsten carbide into molybdenum disulfide, so that this type of film can achieve ultra-low friction and wear in a vacuum environment and have good oxidation resistance.

[0023] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Specifically, as one aspect of the technical solution of the present invention, a radiation-resistant low-friction composite film includes: a titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer sequentially formed on the surface of a substrate;

[0025] Among them, in the direction gradually away from the substrate, the titanium content in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer gradually decreases, the zinc content gradually increases, the molybdenum disulfide content gradually increases, and the tungsten carbide content gradually increases; at the same time, in the direction gradually away from the substrate, zinc, molybdenum disulfide, and tungsten carbide are evenly distributed in the zinc / molybdenum disulfide / tungsten carbide layer.

[0026] In the present invention, Ti, Zn, WC and molybdenum disulfide synergistically achieve the anti-oxidation performance, mechanical properties and tribological properties of the film.

[0027] In some preferred embodiments, the zinc atomic content in the zinc / molybdenum disulfide / tungsten carbide layer is 1.87 to 4.69 at.%.

[0028] In some preferred embodiments, the zinc / molybdenum disulfide / tungsten carbide layer is a multilayer structure formed by a plurality of molybdenum disulfide-zinc composite layers and tungsten carbide layers.

[0029] In some preferred embodiments, the thickness of the titanium transition layer is 100-300 nm.

[0030] In some preferred embodiments, the thickness of the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer is 100-300 nm.

[0031] In some preferred embodiments, the zinc / molybdenum disulfide / tungsten carbide layer has a thickness of 1.2 to 1.6 μm.

[0032] In some preferred embodiments, the composite film has a thickness of 1.7 to 2.0 μm.

[0033] In some preferred embodiments, the substrate is made of 316 steel or single crystal silicon.

[0034] In some preferred embodiments, the friction coefficient of the composite film in a vacuum environment is 0.007 to 0.015, and the wear rate is 1.2 to 1.6×10 -7 mm 3 / N·m.

[0035] In some preferred embodiments, after the composite film is irradiated with atomic oxygen, the friction coefficient in a vacuum environment is 0.006 to 0.013, and the wear rate is 1.3 to 1.6×10 -7 mm 3 / N·m; the conditions for atomic oxygen irradiation include: vacuum degree of 10 -3 ~10 -2 Pa, the irradiation distance is 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0036] The composite film of the present invention has excellent radiation resistance and tribological properties. 21 atoms·cm -2 The vacuum friction coefficient of the film under the atomic oxygen irradiation dose is much lower than 0.01, which can meet the service requirements of spacecraft in the atomic oxygen environment of low-Earth orbit, and provide a scientific basis and theoretical support for the preparation process of molybdenum disulfide-based films.

[0037] Another aspect of an embodiment of the present invention also provides a method for preparing the aforementioned radiation-resistant, low-friction composite film, which comprises: using magnetron sputtering technology to sequentially deposit a titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer on the surface of a substrate, thereby obtaining a radiation-resistant, low-friction composite film.

[0038] In some preferred embodiments, the preparation method specifically includes: using magnetron sputtering technology, using a titanium target as a cathode target material, using an inert gas as a working gas, applying a target current to the titanium target, and applying a negative bias voltage to the substrate, thereby depositing a titanium transition layer on the substrate surface, wherein the target current is 2.0 to 5.0 A, the substrate bias voltage is -50 to -100 V, the working gas flow rate is 12 to 18 sccm, the substrate temperature is 80 to 120 ° C, and the pressure in the reaction chamber is 1.0 to 3.0 × 10 -1 Pa, and the deposition time is 600 to 1200 s.

[0039] Furthermore, the inert gas is argon, but is not limited thereto.

[0040] In some preferred embodiments, the preparation method specifically includes: using magnetron sputtering technology, using titanium target, zinc target, molybdenum disulfide target, and tungsten carbide target as cathode target materials, using inert gas as working gas, applying target current to the titanium target, zinc target, molybdenum disulfide target, and tungsten carbide target, and applying negative bias to the substrate, so as to deposit a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer on the surface of the titanium transition layer; wherein the target current applied to the titanium target gradually decreases from 2.0 to 5.0 A to 0, the target current applied to the zinc target gradually increases from 0 to 0.2 to 1.0 A, the target current applied to the molybdenum disulfide target gradually increases from 0 to 0.8 to 2.0 A, and the target current applied to the tungsten carbide target gradually increases from 0 to 0.6 to 1.0 A, the substrate bias is -30 to -70 V, the flow rate of the working gas is 12 to 18 sccm, the substrate temperature is 80 to 120 ° C, and the pressure of the reaction chamber is 1.0 to 3.0 × 10 -1 Pa, and the deposition time is 600 to 1200 s.

[0041] Furthermore, the inert gas is argon, but is not limited thereto.

[0042] In some preferred embodiments, the preparation method specifically includes: using magnetron sputtering technology, using zinc target, molybdenum disulfide target and tungsten carbide target as cathode target materials, using inert gas as working gas, applying target current to zinc target, molybdenum disulfide target and tungsten carbide target, and applying negative bias to the substrate, so as to deposit zinc / molybdenum disulfide / tungsten carbide layer on the surface of titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer; wherein the target current applied to the zinc target is 0.3-1.0A, the target current applied to the molybdenum disulfide target is 0.8-2.0A, the target current applied to the tungsten carbide target is 0.6-1.0A, the substrate bias is -30--70V, the flow rate of the working gas is 12-18sccm, the substrate temperature is 80-120°C, and the pressure of the reaction chamber is 1.0-3.0×10 -1 Pa, and the deposition time is 6000-8000s.

[0043] Furthermore, the inert gas is argon, but is not limited thereto.

[0044] In some preferred embodiments, the preparation method further comprises: evacuating the reaction chamber to a vacuum degree of 1.0 to 3.0×10 -3 Pa or less, firstly perform plasma etching treatment on the substrate, wherein the plasma etching treatment comprises: applying a bias voltage of -400 to -500 V to the substrate, the substrate temperature is 100 to 150° C., and the etching time is 1200 to 1800 s.

[0045] In some more specific embodiments, the method for preparing the radiation-resistant low-friction composite film (referred to as: Zn-MoS2 / WC film) comprises:

[0046] (1) Using magnetron sputtering technology, inert gas is used as the working gas, and the reaction chamber is evacuated to a vacuum of 1.0 to 3.0 × 10 -3 Pa or less, firstly perform plasma etching treatment on the substrate, the plasma etching treatment comprises: applying a bias voltage of -400 to 500 V to the substrate, the substrate temperature is 100 to 150° C., and the etching time is 1200 to 1800 s.

[0047] (2) magnetron sputtering technology is used, inert gas is used as working gas, target current is applied to the titanium target, and negative bias voltage is applied to the substrate, so as to deposit a titanium transition layer on the substrate surface, wherein the target current is 2.0 to 5.0 A, the substrate bias voltage is -50 to -100 V, so as to deposit a titanium transition layer on the substrate surface, wherein the working gas flow rate is 12 to 18 sccm, the substrate temperature is 80 to 120°C, and the reaction chamber pressure is 1.0 to 3.0×10 -1 Pa, and the deposition time is 600 to 1200 s.

[0048] (3) Magnetron sputtering technology is used, titanium target, zinc target, molybdenum disulfide target and tungsten carbide target are used as cathode target materials, inert gas is used as working gas, target current is applied to the titanium target, zinc target, molybdenum disulfide target and tungsten carbide target, and negative bias is applied to the substrate, so as to deposit a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer on the surface of the titanium transition layer, wherein the target current applied to the titanium target is gradually reduced from 2.0 to 5.0 A to 0, the target current applied to the zinc target is gradually increased from 0 to 0.2 to 1.0 A, the target current applied to the molybdenum disulfide target is gradually increased from 0 to 0.8 to 2.0 A, the target current applied to the tungsten carbide target is gradually increased from 0 to 0.6 to 1.0 A, the substrate bias is -30 to -70 V, the flow rate of the working gas is 12 to 18 sccm, the substrate temperature is 80 to 120 ° C, and the pressure of the reaction chamber is 1.0 to 3.0 × 10 -1 Pa, and the deposition time is 600 to 1200 s.

[0049] (4) magnetron sputtering technology is used, zinc target, molybdenum disulfide target and tungsten carbide target are used as cathode target materials, inert gas is used as working gas, target current is applied to the zinc target, molybdenum disulfide target and tungsten carbide target, and negative bias voltage is applied to the substrate, so as to deposit a multilayer structure of zinc / molybdenum disulfide / tungsten carbide layer on the surface of the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer, wherein the target current applied to the zinc target is 0.3-1.0 A, the target current applied to the molybdenum disulfide target is 0.8-2.0 A, the target current applied to the tungsten carbide target is 0.6-1.0 A, the substrate bias voltage is -30--70 V, the flow rate of the working gas is 12-18 sccm, the substrate temperature is 80-120° C., and the pressure of the reaction chamber is 1.0-3.0×10 -1 Pa, and the deposition time is 6000-8000s.

[0050] Another aspect of the embodiments of the present invention further provides the use of the aforementioned radiation-resistant, low-friction composite film in the field of surface protection of aerospace devices.

[0051] The inventors of this case also conducted the following performance tests on the composite film prepared above:

[0052] The film thickness was tested using a scanning electron microscope, and the test results showed that the film was 1.7 to 2.0 μm.

[0053] Transmission electron microscopy shows that the cross-section of the film is a nano-multilayer structure.

[0054] The hardness and elastic modulus of the film were measured by a nanoindentation system, with a diamond indenter, a penetration depth of 200 nm, and an average value of six points. Test results: The nanohardness of the Zn-MoS2 / WC film of the present invention is greater than 7 GPa.

[0055] Friction and wear test, using CSM friction tester, tribological performance analysis in vacuum environment. CCr15 steel ball is used as counterpart, reciprocating sliding mode is adopted, frequency is 5Hz, track length is 5mm, normal load is 5N, and running distance is 18000 revolutions.

[0056] The friction life test uses a CSM friction tester to perform tribological performance analysis in a vacuum environment. CCr15 steel balls are used as counterparts, and the rotation speed is 1000rpm, the track radius is 6mm, and the normal load is 5N. The test results show that the friction coefficient is less than 0.02 during the entire friction test process, and the friction life exceeds 1 million revolutions.

[0057] In summary, through the above technical solutions, the metal-molybdenum disulfide / ceramic film with a multilayer structure provided by the present invention has good friction and wear performance in a vacuum environment, the friction coefficient is as low as 0.01, and it can operate continuously and stably.

[0058] The atomic oxygen irradiation in the present invention includes: using an electron cyclotron resonance ECR microwave source (MY-1000AD) to generate oxygen plasma, which is converted into a positive oxygen ion beam under the action of an electromagnetic field and accelerated to a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam, whose collision kinetic energy of 5eV is the same as the collision energy of atomic oxygen in low-Earth orbit on the material surface. The atomic oxygen flux of the irradiation test was calibrated by the Kapton-mass loss method to be 1.7×10 16 atoms·cm -2 ·s -1 , and its calibration formula is: f = M / gδst. Among them, f represents the atomic oxygen flux, M, g, δ, s and t represent the mass loss, density, erosion rate, irradiation area and irradiation time of Kapton respectively. In the irradiation test, the flux of atomic oxygen irradiation can be changed by adjusting the flow rate of high-purity oxygen and the microwave power of the microwave source. The vacuum degree of the vacuum chamber is 10 -3 ~10 - 2 Pa, the irradiation distance is about 8-10cm, the gas flow rate is 7-8sccm, and the atomic oxygen irradiation time is 100h.

[0059] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0060] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0061] Example 1

[0062] In this embodiment, the substrate material is 316 steel or single crystal silicon wafer. The Zn-MoS2 / WC-1 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0063] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0064] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0065] (3) Preparation and deposition of Zn-MoS2 / WC-1 thin film, high-purity argon gas was filled into the chamber, Ti target (purity of 99.99at.%), Zn target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%), WC target (purity of 99.99at.%) were arranged and controlled, wherein the Zn target was at position 2, the WC target was at position 1, the sample holder speed was 5rpm, and magnetron sputtering technology was used. The specific steps are as follows:

[0066] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0067] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0068] The sputtering current of the titanium target was gradually reduced from 3.0A to 0A, while the sputtering current of the zinc target was gradually increased from 0 to 0.3A, the sputtering current of the molybdenum disulfide target was gradually increased from 0 to 1.6A, and the sputtering current of the tungsten carbide target was gradually increased from 0 to 0.8A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the gradient transition layer of titanium / zinc / molybdenum disulfide / tungsten carbide deposited on the surface of the titanium transition layer is about 400nm;

[0069] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the zinc target current was kept at 0.3A, the tungsten carbide target current was kept at 0.8A, and the other conditions remained unchanged. The deposition time was 6000s, and a Zn-MoS2 / WC-1 film with a total thickness of 1.88μm was obtained.

[0070] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0071] The following structural performance tests were performed on the Zn-MoS2 / WC-1 film:

[0072] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0073] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0074] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0075] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0076] Figure 1 is a surface SEM image of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention; Figure 2 is a cross-sectional SEM image of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention; Figure 3 is a cross-sectional TEM image of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention; Figure 4 is a graph of hardness and elastic modulus of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention; Figure 5 is a friction coefficient diagram of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention; Figure 6 is a wear rate diagram of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention; Figure 7 This is a friction life diagram of the Zn-MoS2 / WC-1 film prepared in Example 1 of the present invention.

[0077] Example 2

[0078] In the embodiment, the substrate material is 316 steel or a single crystal silicon wafer. The Zn-MoS2 / WC-2 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0079] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0080] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0081] (3) Preparation and deposition of Zn-MoS2 / WC-2 thin film, high-purity argon gas was filled into the chamber, Ti target (purity of 99.99at.%), Zn target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%), WC target (purity of 99.99at.%) were arranged, wherein the Zn target was at position 2, the WC target was at position 1, the sample holder speed was 1.5rpm, and magnetron sputtering technology was used. The specific steps are as follows:

[0082] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0083] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0084] The sputtering current of the titanium target was gradually reduced from 3.0A to 0A, while the sputtering current of the zinc target was gradually increased from 0 to 0.3A, the sputtering current of the molybdenum disulfide target was gradually increased from 0 to 1.6A, and the sputtering current of the tungsten carbide target was gradually increased from 0 to 0.8A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the gradient transition layer of titanium / zinc / molybdenum disulfide / tungsten carbide deposited on the surface of the titanium transition layer is about 400nm;

[0085] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the zinc target current was kept at 0.3A, the tungsten carbide target current was kept at 0.8A, and the other conditions remained unchanged. The deposition time was 6000s, and a Zn-MoS2 / WC-2 film with a total thickness of 1.90μm was obtained.

[0086] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0087] The following structural performance tests were conducted on the Zn-MoS2 / WC-2 film:

[0088] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0089] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0090] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0091] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0092] Example 3

[0093] In the embodiment, the substrate material is 316 steel or single crystal silicon wafer. The Zn-MoS2 / WC-3 thin film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0094] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0095] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0096] (3) Preparation and deposition of Zn-MoS2 / WC-3 thin film, high-purity argon gas was filled into the chamber, Ti target (purity of 99.99at.%), Zn target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%), WC target (purity of 99.99at.%) were arranged, wherein the Zn target was at position 3, the WC target was at position 1, the sample holder speed was 1.5rpm, and magnetron sputtering technology was used. The specific steps are as follows:

[0097] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0098] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0099] The sputtering current of the titanium target was gradually reduced from 3.0A to 0A, while the sputtering current of the zinc target was gradually increased from 0 to 0.3A, the sputtering current of the molybdenum disulfide target was gradually increased from 0 to 1.6A, and the sputtering current of the tungsten carbide target was gradually increased from 0 to 0.8A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the gradient transition layer of titanium / zinc / molybdenum disulfide / tungsten carbide deposited on the surface of the titanium transition layer is about 400nm;

[0100] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the zinc target current was kept at 0.3A, the tungsten carbide target current was kept at 0.8A, and the other conditions remained unchanged. The deposition time was 6000s, and a Zn-MoS2 / WC-3 film with a total thickness of 1.78μm was obtained.

[0101] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0102] The following structural performance tests were performed on the Zn-MoS2 / WC-3 film:

[0103] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0104] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0105] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0106] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0107] Comparative Example 1

[0108] Compared with the embodiment, the difference between this comparative example and the embodiment is that there is no co-doping of Zn and WC elements. In this comparative example, the substrate material is 316 steel or a single crystal silicon wafer. A pure MoS2 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0109] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0110] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0111] (3) Preparation and deposition of MoS2 thin film, high-purity argon gas is filled into the chamber, Ti target (purity of 99.99at.%) and MoS2 target (purity of 99.9at.%) are arranged and controlled, and magnetron sputtering technology is used. The specific steps are as follows:

[0112] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0113] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0114] The sputtering current of the titanium target was gradually reduced to 0 A, and the sputtering current of the molybdenum disulfide target was gradually increased to 1.6 A. The working gas was Ar, the gas flow rate was 16 sccm, the substrate bias was -50 V, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and the thickness of the titanium / molybdenum disulfide gradient transition layer deposited on the surface of the titanium transition layer is about 400nm;

[0115] The sputtering current of the molybdenum disulfide target was kept at 1.6 A, the other conditions remained unchanged, the deposition time was 6000 s, and the total thickness of the MoS2 film obtained was 2.72 μm.

[0116] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0117] The MoS2 film after the above deposition treatment was subjected to the following structural performance tests:

[0118] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0119] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0120] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0121] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0122] Comparative Example 2

[0123] Compared with the embodiment, the difference between this comparative example and the embodiment is that there is no doping of Zn element. In this comparative example, the substrate material is 316 steel or single crystal silicon wafer. The MoS2 / WC film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0124] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0125] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10-3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0126] (3) Preparation and deposition of MoS2 / WC thin film, high-purity argon gas is filled into the chamber, Ti target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%), WC target (purity of 99.99at.%) are arranged and controlled, and magnetron sputtering technology is used. The specific steps are as follows:

[0127] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0128] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0129] The sputtering current of the titanium target was gradually reduced to 0 A, and the sputtering current of the tungsten carbide target was gradually increased to 0.8 A and the sputtering current of the molybdenum disulfide target was gradually increased to 1.6 A. The working gas was Ar, the gas flow rate was 16 sccm, the substrate bias was -50 V, the deposition substrate temperature was 100 °C, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the titanium / molybdenum disulfide / tungsten carbide gradient transition layer deposited on the surface of the titanium transition layer is about 400nm;

[0130] The sputtering current of the molybdenum disulfide target was kept at 1.6 A, the sputtering current of the tungsten carbide target was kept at 0.8 A, and the other conditions remained unchanged. The deposition time was 6000 s, and the total thickness of the MoS2 / WC film obtained was 2.32 μm.

[0131] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0132] The MoS2 / WC film after the above deposition treatment was subjected to the following structural performance tests:

[0133] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0134] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0135] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0136] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0137] Comparative Example 3

[0138] Compared with Example 1, this comparative example is different in that there is no WC doping. In this comparative example, the substrate material is 316 steel or single crystal silicon wafer. The MoS2 / Zn film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0139] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0140] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0141] (3) Preparation and deposition of MoS2 / Zn thin film: high-purity argon gas is filled into the chamber, Ti target (purity of 99.99 at.%), MoS2 target (purity of 99.9 at.%), and Zn target (purity of 99.99 at.%) are arranged and controlled, and magnetron sputtering technology is used. The specific steps are as follows:

[0142] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0143] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0144] The sputtering current of the titanium target was gradually reduced to 0 A, while the sputtering current of the Zn target was gradually increased to 0.3 A and the sputtering current of the molybdenum disulfide target was gradually increased to 1.6 A. The working gas was Ar, the gas flow rate was 16 sccm, the substrate bias was -50 V, the deposition substrate temperature was 100 °C, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the titanium / molybdenum disulfide / zinc gradient transition layer deposited on the surface of the titanium transition layer is about 400nm;

[0145] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the sputtering current of the zinc target was kept at 0.3A, and the other conditions remained unchanged. The deposition time was 6000s, and the total thickness of the MoS2 / Zn film obtained was 2.37μm.

[0146] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0147] The MoS2 / Zn film after the above deposition treatment was subjected to the following structural performance tests:

[0148] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0149] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0150] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0151] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0152] Comparative Example 4

[0153] Compared with Example 1, this comparative example lacks the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer. In this comparative example, the substrate material is 316 steel or a single crystal silicon wafer. The Zn-MoS2 / WC-4 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0154] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0155] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0156] (3) Preparation and deposition of Zn-MoS2 / WC-4 thin film, high-purity argon gas was filled into the chamber, Ti target (purity of 99.99at.%), Zn target (purity of 99.99at.%), MoS2 target (purity of 99.9at.%), WC target (purity of 99.99at.%) were arranged, wherein the Zn target was at position 2, the WC target was at position 1, the sample holder speed was 5rpm, and magnetron sputtering technology was used. The specific steps are as follows:

[0157] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0158] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0159] The sputtering current of the zinc target was 0.3A, the sputtering current of the molybdenum disulfide target was 1.6A, and the sputtering current of the tungsten carbide target was 0.8A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 6000s, and the Zn-MoS2 / WC-4 film is prepared with a total thickness of 1.80μm.

[0160] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0161] The following structural performance tests were conducted on the Zn-MoS2 / WC-4 film:

[0162] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0163] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0164] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0165] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0166] Comparative Example 5

[0167] Compared with Example 1, the content of zinc in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer in the direction away from the substrate is constant. In this comparative example, the substrate material is 316 steel or a single crystal silicon wafer. The Zn-MoS2 / WC-5 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0168] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0169] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0170] (3) Preparation and deposition of Zn-MoS2 / WC-5 thin film, high-purity argon gas is filled into the cavity, Ti target (purity of 99.99at.%) and MoS2 target (purity of 99.9at.%) are used for layout and control, and magnetron sputtering technology is used. The specific steps are as follows:

[0171] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0172] The titanium target sputtering current was 3.0A, the substrate bias voltage was -70V, the working gas was Ar, the gas flow rate was 16sccm, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0173] The sputtering current of the titanium target was gradually reduced from 3.0A to 0A, the sputtering current of the zinc target was maintained at 0.3A, the sputtering current of the molybdenum disulfide target was gradually increased from 0 to 1.6A, and the sputtering current of the tungsten carbide target was gradually increased from 0 to 0.8A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the gradient transition layer of titanium / zinc / molybdenum disulfide / tungsten carbide deposited on the surface of the titanium transition layer is about 400nm;

[0174] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the zinc target current was kept at 0.3A, the tungsten carbide target current was kept at 0.8A, and the other conditions remained unchanged. The deposition time was 6000s, and a Zn-MoS2 / WC-5 film with a total thickness of 1.86μm was obtained.

[0175] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0176] The Zn-MoS2 / WC-5 film after the above deposition treatment was subjected to the following structural performance tests:

[0177] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0178] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0179] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0180] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0181] Comparative Example 6

[0182] Compared with Example 1, the content of molybdenum disulfide in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer in the direction away from the substrate is unchanged. In this comparative example, the substrate material is 316 steel or a single crystal silicon wafer. The Zn-MoS2 / WC-6 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0183] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0184] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0185] (3) Preparation and deposition of Zn-MoS2 / WC-6 thin film, high-purity argon gas is filled into the cavity, Ti target (purity of 99.99at.%) and MoS2 target (purity of 99.9at.%) are used for layout and control, and magnetron sputtering technology is used. The specific steps are as follows:

[0186] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0187] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0188] The sputtering current of the titanium target was gradually reduced from 3.0A to 0A, the sputtering current of the zinc target was gradually increased from 0 to 0.3A, the sputtering current of the molybdenum disulfide target was maintained at 1.6A, and the sputtering current of the tungsten carbide target was gradually increased from 0 to 0.8A. The working gas was Ar, the gas flow rate was 16sccm, the substrate bias was -50V, the deposition substrate temperature was 100℃, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the gradient transition layer of titanium / zinc / molybdenum disulfide / tungsten carbide deposited on the surface of the titanium transition layer is about 400nm;

[0189] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the zinc target current was kept at 0.3A, the tungsten carbide target current was kept at 0.8A, and the other conditions remained unchanged. The deposition time was 6000s, and a Zn-MoS2 / WC-6 film with a total thickness of 1.83μm was obtained.

[0190] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0191] The Zn-MoS2 / WC-6 film after the above deposition treatment was subjected to the following structural performance tests:

[0192] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0193] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0194] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0195] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0196] Comparative Example 7

[0197] Compared with Example 1, the content of tungsten carbide in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer in the direction away from the substrate is unchanged. In this comparative example, the substrate material is 316 steel or a single crystal silicon wafer. The Zn-MoS2 / WC-7 film is prepared on the substrate surface by magnetron sputtering technology, which mainly includes the following steps:

[0198] (1) The surface of the substrate is mechanically polished, the substrate material is placed in an acetone solution for ultrasonic cleaning for 30 minutes, dried with nitrogen, placed in an anhydrous ethanol solution for ultrasonic cleaning for 30 minutes, and dried with nitrogen.

[0199] (2) Place the cleaned substrate into the magnetron sputtering chamber and evacuate it to a vacuum degree of less than 5×10 -3 Pa, and then sputter clean the target for 30 minutes, with the substrate temperature being 100-150°C.

[0200] (3) Preparation and deposition of Zn-MoS2 / WC-7 thin film, high-purity argon gas is filled into the cavity, Ti target (purity of 99.99at.%) and MoS2 target (purity of 99.9at.%) are used, and magnetron sputtering technology is used. The specific steps are as follows:

[0201] Plasma etching, a bias voltage of -500 V was applied to the substrate, the program running time was 30 min, and the substrate temperature was 100 °C.

[0202] The titanium target sputtering current was 3.0 A, the substrate bias voltage was -70 V, the working gas was Ar, the gas flow rate was 16 sccm, the deposition substrate temperature was 100 °C, and the pressure was 1.3 × 10 -1 Pa, the deposition time is 600s, and a titanium transition layer with a thickness of about 200nm is deposited on the substrate surface;

[0203] The sputtering current of the titanium target was gradually reduced from 3.0 A to 0 A, the sputtering current of the zinc target was gradually increased from 0 to 0.3 A, the sputtering current of the molybdenum disulfide target was increased from 0 to 1.6 A, and the sputtering current of the tungsten carbide target was maintained at 0.8 A. The working gas was Ar with a gas flow rate of 16 sccm, the substrate bias was -50 V, the deposition substrate temperature was 100 °C, and the pressure was 1.3×10 -1 Pa, the deposition time is 600s, and the thickness of the gradient transition layer of titanium / zinc / molybdenum disulfide / tungsten carbide deposited on the surface of the titanium transition layer is about 400nm;

[0204] The sputtering current of the molybdenum disulfide target was kept at 1.6A, the zinc target current was kept at 0.3A, the tungsten carbide target current was kept at 0.8A, and the other conditions remained unchanged. The deposition time was 6000s, and a Zn-MoS2 / WC-7 film with a total thickness of 1.87μm was obtained.

[0205] The conditions of the atomic oxygen irradiation test are as follows: an electron cyclotron resonance (ECR) microwave source (MY-1000AD) is used to generate oxygen plasma, which is transformed into a positive oxygen ion beam under the action of an electromagnetic field and accelerated toward a negatively charged metal plate. After colliding with the metal plate, the positive oxygen ions are neutralized by the negative charge and rebound to form a neutral atomic oxygen beam with a collision kinetic energy of 5 eV. During the irradiation test, the vacuum degree of the vacuum chamber was 10 -3 ~10 -2 Pa, the irradiation distance is about 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms·cm -2 ·s -1 , the atomic oxygen irradiation time is 100h.

[0206] The Zn-MoS2 / WC-7 film after the above deposition treatment was subjected to the following structural performance tests:

[0207] (1) Surface morphology test: Scanning electron microscopy was used to measure the surface cross-sectional morphology and film thickness of the film.

[0208] (2) Structural testing: The microstructure of the film cross section was observed using a transmission electron microscope.

[0209] (3) Mechanical properties test: The hardness and elastic modulus of the film were measured using a nanoindenter system.

[0210] (4) Friction and wear performance test under vacuum environment: CSM friction tester was used to perform tribological performance analysis under vacuum environment. CCr15 steel ball was used as the dual ball, reciprocating sliding mode was adopted, the frequency was 5 Hz, the track length was 5 mm, the operation was 18,000 revolutions, and the normal load was 5 N.

[0211] The five films prepared by different processes in Examples 1-3 and Comparative Examples 1-7 are named as follows: Zn-MoS2 / WC-1, Zn-MoS2 / WC-2, Zn-MoS2 / WC-3, MoS2, MoS2 / WC, MoS2 / Zn, Zn-MoS2 / WC-4, Zn-MoS2 / WC-5, Zn-MoS2 / WC-6, Zn-MoS2 / WC-7. The content of each element is shown in Table 1 below.

[0212] Table 1: Composition parameters of film samples (outermost layer) in Examples 1-3 and Comparative Examples 1-7

[0213]

[0214] It can be seen from Table 1 that the main body of the deposited film is MoS2, which meets the requirements of lubricating functional film.

[0215] The thickness and friction coefficient of the films of Zn-MoS2 / WC-1, Zn-MoS2 / WC-2, Zn-MoS2 / WC-3, MoS2, MoS2 / WC, MoS2 / Zn, Zn-MoS2 / WC-4, Zn-MoS2 / WC-5, Zn-MoS2 / WC-6, and Zn-MoS2 / WC-7 in Examples 1-3 and Comparative Examples 1-7 are shown in Table 2. As can be seen from Table 2, the film of Example 1 has the best friction coefficient in a vacuum environment.

[0216] Table 2: Thickness and vacuum average friction coefficient of film samples in Examples 1-3 and Comparative Examples 1-7

[0217]

[0218]

[0219] The hardness, elastic modulus and bonding strength of the Zn-MoS2 / WC-1, Zn-MoS2 / WC-2, Zn-MoS2 / WC-3, MoS2, MoS2 / WC, MoS2 / Zn, Zn-MoS2 / WC-4, Zn-MoS2 / WC-5, Zn-MoS2 / WC-6 and Zn-MoS2 / WC-7 films in Examples 1-3 and Comparative Examples 1-7 are shown in Table 3. As can be seen from Table 3, the film of Example 1 has excellent mechanical properties.

[0220] Table 3: Hardness, elastic modulus and bonding strength of film samples in Examples 1-3 and Comparative Examples 1-7

[0221]

[0222] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0223] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A radiation-resistant, low-friction composite film, characterized in that: include: A titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer are sequentially formed on the surface of the substrate; Among them, in the direction gradually away from the substrate, the titanium content in the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer gradually decreases, the zinc content gradually increases, the molybdenum disulfide content gradually increases, and the tungsten carbide content gradually increases; at the same time, in the direction gradually away from the substrate, zinc, molybdenum disulfide, and tungsten carbide are evenly distributed in the zinc / molybdenum disulfide / tungsten carbide layer.

2. The composite film according to claim 1, characterized in that: The zinc atomic content in the zinc / molybdenum disulfide / tungsten carbide layer is 1.87 to 4.69 at.%; And / or, the zinc / molybdenum disulfide / tungsten carbide layer is a multilayer structure formed by a plurality of molybdenum disulfide-zinc composite layers and tungsten carbide layers.

3. The composite film according to claim 1, characterized in that: The thickness of the titanium transition layer is 100-300 nm; and / or the thickness of the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer is 100-300 nm; and / or the thickness of the zinc / molybdenum disulfide / tungsten carbide layer is 1.2-1.6 μm; and / or the thickness of the composite film is 1.7-2.0 μm; And / or, the material of the substrate includes 316 steel or single crystal silicon.

4. The composite film according to claim 1, characterized in that: The friction coefficient of the composite film in a vacuum environment is 0.007-0.015, and the wear rate is 1.2-1.6×10 -7 mm 3 / N·m; And / or, after the composite film is irradiated with atomic oxygen, the friction coefficient in a vacuum environment is 0.006-0.013, and the wear rate is 1.3-1.6×10 -7 mm 3 / N·m; the conditions for atomic oxygen irradiation include: vacuum degree of 10 -3 10 -2 Pa, the irradiation distance is 8-10 cm, the gas flow rate is 7-8 sccm, and the atomic oxygen flux is 1.7×10 16 atoms.cm -2 .s -1 , the atomic oxygen irradiation time is 100h.

5. The method for preparing a radiation-resistant low-friction composite film according to any one of claims 1 to 4, characterized in that: include: A titanium transition layer, a titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer and a zinc / molybdenum disulfide / tungsten carbide layer are sequentially deposited on the substrate surface by magnetron sputtering technology to obtain a radiation-resistant, low-friction composite film.

6. The preparation method according to claim 5, characterized in that: Specifically include: The magnetron sputtering technology is used, with titanium target as cathode target material, inert gas as working gas, target current applied to the titanium target, and negative bias applied to the substrate, so as to deposit and form a titanium transition layer on the substrate surface, wherein the target current is 2.0-5.0A, the substrate bias is -50--100V, the working gas flow rate is 12-18sccm, the substrate temperature is 80-120℃, and the pressure in the reaction chamber is 1.0-3.0×10 -1 Pa, and the deposition time is 600 to 1200 s.

7. The preparation method according to claim 5, characterized in that: Specifically include: The invention adopts magnetron sputtering technology, uses titanium target, zinc target, molybdenum disulfide target and tungsten carbide target as cathode target materials, uses inert gas as working gas, applies target current to titanium target, zinc target, molybdenum disulfide target and tungsten carbide target, and applies negative bias voltage to substrate, so as to deposit titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer on the surface of the titanium transition layer; wherein, the target current applied to the titanium target gradually decreases from 2.0 to 5.0 A to 0, the target current applied to the zinc target gradually increases from 0 to 0.2 to 1.0 A, the target current applied to the molybdenum disulfide target gradually increases from 0 to 0.8 to 2.0 A, the target current applied to the tungsten carbide target gradually increases from 0 to 0.6 to 1.0 A, the substrate bias voltage is -30 to -70 V, the flow rate of working gas is 12 to 18 sccm, the substrate temperature is 80 to 120° C., and the pressure of the reaction chamber is 1.0 to 3.0×10 - 1 Pa, and the deposition time is 600 to 1200 s.

8. The preparation method according to claim 5, characterized in that: Specifically include: The magnetron sputtering technology is adopted, a zinc target, a molybdenum disulfide target and a tungsten carbide target are used as cathode target materials, an inert gas is used as a working gas, a target current is applied to the zinc target, the molybdenum disulfide target and the tungsten carbide target, and a negative bias voltage is applied to the substrate, so that a zinc / molybdenum disulfide / tungsten carbide layer is deposited on the surface of the titanium / zinc / molybdenum disulfide / tungsten carbide gradient transition layer; wherein the target current applied to the zinc target is 0.3-1.0A, the target current applied to the molybdenum disulfide target is 0.8-2.0A, the target current applied to the tungsten carbide target is 0.6-1.0A, the substrate bias voltage is -30--70V, the flow rate of the working gas is 12-18sccm, the substrate temperature is 80-120°C, and the pressure of the reaction chamber is 1.0-3.0×10 -1 Pa, and the deposition time is 6000-8000s.

9. The preparation method according to claim 5, characterized in that: Also includes: The vacuum degree of the reaction chamber was reduced to 1.0-3.0×10 -3 Pa or less, firstly perform plasma etching treatment on the substrate, wherein the plasma etching treatment comprises: applying a bias voltage of -400 to -500 V to the substrate, the substrate temperature is 100 to 150° C., and the etching time is 1200 to 1800 s.