Humidity-responsive variable stiffness material and preparation method thereof
By using PVAm and PEI blending in humidity-responsive materials, using changes in crystallization and hydrogen bonds, the extremely stiffness change of the material between drying and hygroscopic states is achieved, and the problem of insufficient stiffness change in existing materials is solved. It has strong Adhesion and shape memory capability, suitable for a variety of applications.
Patent Information
- Application Number
- CN202411134067.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-19
AI Technical Summary
When existing humidity-responsive materials keep the volume and solid state unchanged, the degree of stiffness changes is insufficient and cannot meet the actual application needs.
Polyethylene amine (PVAm) and polyethyleneimine (PEI) are blended to form a material with a large stiffness change through the combined action of crystallization and hydrogen bonding. The specific method is to prepare PVAm/PEI variable stiffness materials according to a specific weight ratio, and use water molecules to destroy crystallization and hydrogen bonds to achieve efficient stiffness changes.
Achieve 71,000 times change between high rigidity (1560.85MPa) of the material during drying and low rigidity (0.022MPa) after hygroscopicity, has strong adhesion, shape locking and shape memory capabilities, can carry external loads and be drying After quickly recovering the shape.
Smart Images

Figure CN118931181A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a humidity-responsive variable-rigidity material and a preparation method thereof, and belongs to the field of intelligent polymer materials. Background Art
[0002] Variable stiffness materials are intelligent polymer materials that change their hardness and softness through some kind of stimulation. They have been widely used in soft robots, intelligent adhesives, biomedical minimally invasive devices and optoelectronic devices. At present, variable stiffness materials are mainly prepared through light, electricity, magnetism, temperature and pressure stimulation, and the stiffness change range is usually within 10,000 times (Park, Sungjune, et al. "Ultrastretchable elastic shape memory fibers with electrical conductivity." Advanced Science 6.21(2019):1901579; Zheng, Xiaoyang, et al. "Minimal-surface-based multiphase metamaterials with highly variablestiffness." Materials&Design 237(2024):112548.).
[0003] Compared with stimuli such as light, electricity, magnetism, temperature and pressure, humidity comes from the air and is an environmentally friendly, non-toxic, low-cost and inexhaustible stimulus source. However, traditional humidity-responsive materials still have shortcomings in achieving stiffness changes. For example, they swell significantly or dissolve into liquid when absorbing moisture; or after absorbing moisture, although the volume and solid state remain unchanged, the degree of stiffness change is small (10 to 100 times), which cannot meet practical applications. Therefore, it is still challenging to achieve materials with large stiffness changes through humidity while keeping the volume and solid state unchanged. Summary of the invention
[0004] [Technical issues]
[0005] In view of the defects and shortcomings of the prior art, the technical problem to be solved by the present invention is that, through humidity stimulation, when the material maintains the volume and solid state unchanged, the degree of stiffness change is insufficient.
[0006] [Technical solution]
[0007] In order to solve the above technical problems, the present invention provides a humidity-responsive variable stiffness material and a preparation method thereof. The humidity-responsive PVAm / PEI variable stiffness material of the present invention specifically uses polyvinylamine (PVAm) as a polymer matrix. Since each repeating unit of polyvinylamine has a primary amine group on the side chain, the structure is regular, and the intramolecular hydrogen bonds between the primary amine groups cause the polyvinylamine molecular chain to fold in order to form a crystalline region, which has good rigidity; the branched structure of polyethyleneimine (PEI) is blended with the polyvinylamine polymer matrix, and the polyethyleneimine and the polyvinylamine form intermolecular hydrogen bonds, which can increase the crystallinity and hydrogen bond association of the PVAm / PEI variable stiffness material at the same time, and realize a material with a large change in stiffness. Due to the combined effect of crystallization and hydrogen bonding, the PVAm / PEI variable stiffness material has a strong rigidity (1560.85MPa) in a dry state; after moisture absorption, the water molecules destroy the original crystallization and hydrogen bonding, so that the stiffness of the material becomes 0.022MPa, and the degree of change is as high as 71,000 times.
[0008] In order to achieve the above object, the present invention provides a humidity-responsive PVAm / PEI variable stiffness material, wherein the PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 6 to 9.5 parts of polyvinylamine (PVAm), 0.5 to 4 parts of polyethyleneimine (PEI), and 90 parts of water.
[0009] In one embodiment of the present invention, the PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 8 to 9.5 parts of polyethylene amine, 0.5 to 2 parts of polyethylene imine, and 90 parts of water.
[0010] In one embodiment of the present invention, the PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 8 to 8.5 parts of polyethylene amine, 1.5 to 2 parts of polyethylene imine, and 90 parts of water.
[0011] In one embodiment of the present invention, the PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 8.5 parts of polyethylene amine, 1.5 parts of polyethylene imine, and 90 parts of water.
[0012] In one embodiment of the present invention, the molecular weight Mw of the polyvinylamine is 1 million to 3 million, preferably 3 million; the molecular weight Mw of the polyethyleneimine is 10,000 to 50,000, preferably 25,000.
[0013] Another object of the present invention is to provide a method for preparing the humidity-responsive PVAm / PEI variable stiffness material described above, the preparation method specifically comprising the following steps:
[0014] Polyethylene amine and polyethylene imine are mixed with water according to the weight ratio to obtain a composite solution, and then the composite solution is poured into a mold, dried, and demolded to obtain a humidity-responsive PVAm / PEI variable stiffness material.
[0015] In one embodiment of the present invention, the mass percentage of the polyethyleneimine is 5-40%, and the mass percentage of the polyethyleneimine is calculated relative to the sum of the polyethyleneamine and the polyethyleneimine; preferably, it is 15-20%.
[0016] In one embodiment of the present invention, the drying condition is 40-60° C., 8-24 h; preferably 60° C., 12 h.
[0017] The third object of the present invention is to provide an application of the above-mentioned PVAm / PEI variable stiffness material in smart adhesion, shape locking and shape memory.
[0018] The fourth object of the present invention is to provide a PVAm / PEI composite material with shape memory, wherein the PVAm / PEI composite material with shape memory is composed of the following raw materials in parts by weight: 6 to 9.5 parts of polyethylene amine, 0.5 to 4 parts of polyethylene imine, and 90 parts of water.
[0019] In one embodiment of the present invention, the PVAm / PEI composite material is composed of the following raw materials in parts by weight: 8 to 9.5 parts of polyvinylamine, 0.5 to 2 parts of polyethyleneimine, and 90 parts of water.
[0020] In one embodiment of the present invention, the PVAm / PEI composite material is composed of the following raw materials in parts by weight: 8 to 8.5 parts of polyethylene amine, 1.5 to 2 parts of polyethylene imine, and 90 parts of water.
[0021] In one embodiment of the present invention, the PVAm / PEI composite material is composed of the following raw materials in parts by weight: 8.5 parts of polyvinylamine, 1.5 parts of polyethyleneimine, and 90 parts of water.
[0022] In one embodiment of the present invention, the molecular weight Mw of the polyvinylamine is 1 million to 3 million, preferably 3 million; the molecular weight Mw of the polyethyleneimine is 10,000 to 50,000, preferably 25,000.
[0023] Beneficial effects:
[0024] (1) The present invention prepares PVAm / PEI variable stiffness material by a one-step method, which is low in cost, fast in speed, energy-saving and environmentally friendly; and the obtained PVAm / PEI variable stiffness material has a strong humidity response performance. The Young's modulus of the material is 1560.85MPa when dry, and the Young's modulus after reaching moisture absorption equilibrium is 0.022MPa, and the degree of stiffness change is as high as 71,000 times.
[0025] (2) The PVAm / PEI variable stiffness material of the present invention also has strong adhesion and can be formed into various complex shapes, and can be formed into the desired shape by heating to meet different needs; the soft variable stiffness material can completely replicate the details and lock them by removing humidity, and can even be changed from simple shapes such as squares and triangles to complex five-pointed star shapes. 4 Shape-locked composites can carry a certain external load over an order of magnitude; exhibit strong load-bearing capacity, shape memory, and can be re-locked into complex 3D shapes due to their 2D stretchability.
[0026] (3) Since the stiffness of the PVAm / PEI variable stiffness material can change rapidly and continuously, the hygroscopic material can easily support a weight of approximately 1.7 kg by adhering to a plastic bottle cap and drying quickly. The PVAm / PEI composite material can rapidly change its stiffness, deform in a flexible and controllable manner, and quickly recover its shape memory and lock. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The polymer network and physical picture of the humidity-responsive PVAm / PEI variable stiffness material prepared in Example 3 of the present invention; (a) Schematic diagram of the PVAm / PEI polymer network; (b) Schematic diagram of the humidity-triggered PVAm / PEI variable stiffness material switching between rigid and soft states;
[0028] Figure 2 Characterization diagrams of the crystallinity and hydrogen bonding degree of the humidity-responsive PVAm / PEI variable stiffness materials prepared in the embodiments of the present invention and the comparative examples; (a) XRD results of different PVAm / PEI variable stiffness materials in a dry state and (b) their corresponding crystallinity data diagrams; (c) XRD results of PVAm / PEI variable stiffness materials at 2900-3700 cm -1 Infrared spectral curves in the range of 1560-1700cm and (d) their corresponding hydrogen bond association degree data diagram; (e) PVAm / PEI variable stiffness material in the range of 1560-1700cm -1 IR spectra at (a) and (b) their corresponding hydrogen bonding degree data diagrams;
[0029] Figure 3The moisture absorption data of the PVAm / PEI variable stiffness materials of the present invention with different ratios at different relative humidity (RH) are shown; (a) 25°C, 25% RH; (b) 25°C, 55% relative humidity; (c) 25°C, 75% relative humidity;
[0030] Figure 4 The stress-strain curves of the PVAm / PEI variable stiffness materials with different ratios of the present invention at 75% RH and different moisture absorption times; (a) 0 minutes, (b) 10 minutes, (c) 20 minutes, (d) 30 minutes, (e) 60 minutes, (f) 120 minutes;
[0031] Figure 5 Mechanism characterization diagram of humidity-responsive PVAm / PEI variable stiffness material prepared in Example 3 of the present invention; (a) XRD of 15% PVAm / PEI variable stiffness material; (b) crystallinity data diagram at different moisture absorption times; (c) physical diagram of the change in transparency of variable stiffness material before and after moisture absorption; (d) in-situ infrared one-dimensional spectrum diagram of 15% PVAm / PEI variable stiffness material at 20-80°C; (d) measured at 1750–1500cm –1 Two-dimensional synchronous infrared correlation spectrum of 15% PVAm / PEI variable stiffness material under different wave numbers; (e) synchronous spectrum; (f) two-dimensional correlation spectrum of asynchronous spectrum; (g) molecular simulation and binding energy calculation data of PVAm chain, PEI chain and water molecule;
[0032] Figure 6 The application effect diagram of the humidity-responsive PVAm / PEI variable stiffness material prepared in Example 3 of the present invention in intelligent adhesion, shape locking and shape memory; (a) The variable stiffness material is reconfigured into a load-bearing 3D shape. After heating and water volatilization, the 3D shape is locked, and after absorbing moisture, it returns to its original state; (b) The adhesion performance effect diagram of the variable stiffness material; (c) The actual picture of the angle change of 15% PVAm / PEI variable stiffness material after moisture absorption for different time periods at 25°C and 75% relative humidity. DETAILED DESCRIPTION
[0033] The preferred embodiments of the present invention are described below. It should be understood that the embodiments are for better explaining the present invention and are not used to limit the present invention.
[0034] The present invention relates to a testing method
[0035] The crystallinity of PVAm / PEI variable stiffness materials was characterized by X-ray diffraction (XRD);
[0036] The hydrogen bonding degree of PVAm / PEI variable stiffness materials was characterized by Fourier transform infrared spectroscopy (FTIR);
[0037] The mechanical properties of PVAm / PEI variable stiffness materials were tested by a universal tensile testing machine;
[0038] After 2 hours at 25°C and 75% RH, the samples were subjected to tensile testing. The stress-strain curve can be divided into two regions - the elastic region, in which the curve is linear, and the plastic region. In the elastic region, the stress-strain curve of most materials is a straight line. This means that the strain is proportional to the applied stress. Hooke's law gives the relationship between stress and strain in this linear elastic region. The ratio between stress and strain is called Young's modulus, also called elastic modulus. Young's modulus (E = stress / strain) is used as a measure of the stiffness of variable stiffness materials.
[0039] The raw materials involved in the embodiments of the present invention and the comparative examples are:
[0040] Polyethylene amine, molecular weight Mw 3 million.
[0041] Polyethyleneimine, molecular weight Mw 25,000.
[0042] Example 1
[0043] A humidity-responsive PVAm / PEI variable stiffness material, the preparation method of which is as follows:
[0044] Take 9.5 parts of polyethyleneamine and 0.5 parts of polyethyleneimine, and then prepare a solution with 90 parts of water, each part is calculated as 1 g. The solution is inverted on a polystyrene culture dish and dried at 60°C for 12 hours to obtain a humidity-responsive PVAm / PEI variable stiffness material.
[0045] Example 2
[0046] A humidity-responsive PVAm / PEI variable stiffness material, the preparation method of which is as follows:
[0047] Take 9 parts of polyethyleneamine and 1 part of polyethyleneimine, and then prepare a solution with 90 parts of water, each part is calculated as 1g, the solution is inverted on a polystyrene culture dish, and dried at 60°C for 12 hours to obtain a humidity-responsive PVAm / PEI variable stiffness material.
[0048] Example 3
[0049] A humidity-responsive PVAm / PEI variable stiffness material, the preparation method of which is as follows:
[0050] Take 8.5 parts of polyethyleneamine and 1.5 parts of polyethyleneimine, and then prepare a solution with 90 parts of water, each part is calculated as 1g. The solution is inverted on a polystyrene culture dish and dried at 60°C for 12 hours to obtain a humidity-responsive PVAm / PEI variable stiffness material.
[0051] Example 4
[0052] A humidity-responsive PVAm / PEI variable stiffness material, the preparation method of which is as follows:
[0053] Take 8 parts of polyethyleneamine and 2 parts of polyethyleneimine, and then prepare a solution with 90 parts of water, each part is calculated as 1g, the solution is inverted on a polystyrene culture dish, and dried at 60°C for 12 hours to obtain a humidity-responsive PVAm / PEI variable stiffness material.
[0054] Example 5
[0055] A humidity-responsive PVAm / PEI variable stiffness material, the preparation method of which is as follows:
[0056] Take 6 parts of polyethyleneamine and 4 parts of polyethyleneimine, and then prepare a solution with 90 parts of water, each part is calculated as 1g, the solution is inverted on a polystyrene culture dish, and dried at 60°C for 12 hours to obtain a humidity-responsive PVAm / PEI variable stiffness material.
[0057] Comparative Example 1
[0058] The only difference from Example 3 is that polyethyleneimine is omitted, and other conditions and parameters are the same as those in Example 3.
[0059] Comparative Example 2
[0060] The only difference from Example 3 is that polyvinylamine is omitted, and other conditions and parameters are the same as those in Example 3.
[0061] Comparative Example 3
[0062] The only difference from Example 3 is that 4 parts of polyvinylamine and 6 parts of polyethyleneimine are used, and other parameters and conditions are the same as those in Example 3.
[0063] Comparative Example 4
[0064] The difference from Example 3 is that polyethyleneimine is replaced by chitosan, and other conditions and parameters are the same as those in Example 3.
[0065] Comparative Example 5
[0066] The only difference from Example 3 is that polyethyleneimine is replaced by polyvinyl alcohol (Mw=23000), and other conditions and parameters are the same as those in Example 3.
[0067] Results Performance Analysis
[0068] Figure 1The polymer network and physical picture of the humidity-responsive variable stiffness material prepared in Example 3; (a) Schematic diagram of the PVAm / PEI polymer network with crystallization and hydrogen bonding; (b) The humidity-triggered PVAm / PEI variable stiffness material switches between rigid and soft states.
[0069] Schematic diagram of polymer network of PVAm / PEI variable stiffness material Figure 1 As shown. In the dry state, the PVAm / PEI variable stiffness material exhibits rigidity due to the crystalline regions within the PVAm molecules (intramolecular hydrogen bonds between the in-situ amine groups on PVAm) and the intermolecular hydrogen bonds between the tightly cross-linked amine groups between PVAm and PEI. After absorbing moisture, the crystalline regions and intermolecular hydrogen bonds of PVAm are destroyed by water molecules, causing the PVAm / PEI variable stiffness material to change from rigid to soft and bendable. When the humidity is removed, the intramolecular hydrogen bonds reform, driving the PVAm molecular chains to fold to form crystalline regions; at the same time, the intermolecular hydrogen bonds between PVAm and PEI are also reconstructed. Therefore, the PVAm / PEI variable stiffness material returns from softness to its original rigid state ( Figure 1 a). These optical images show the stiffness changes of PVAm / PEI variable stiffness materials in dry and wet states, such as Figure 1 b. When absorbing moisture, the PVAm / PEI variable stiffness material becomes soft and flexible; it can easily change shape and quickly return to its initial state after twisting and folding. When the PVAm / PEI variable stiffness material dries, it breaks after twisting the angle and cannot return to its initial state. It is worth noting that these "rigid" and "soft" states can be quickly transformed back to the expected rigid state according to individual needs and basic stimulus-response conditions.
[0070] Figure 2 Characterization of the crystallinity and hydrogen bonding degree of the humidity-responsive variable stiffness material prepared by the present invention. (a) XRD results of different PVAm / PEI variable stiffness materials in dry state and (b) their corresponding crystallinity; (c) XRD results of PVAm / PEI variable stiffness materials at 2900-3700 cm -1 Infrared spectral curves in the range of (d) their corresponding hydrogen bonding degree; (e) PVAm / PEI variable stiffness material in the range of 1560-1700cm -1 Infrared spectral curves at (f) and their corresponding hydrogen bonding degrees.
[0071] Five PVAm / PEI materials, 5% PEI, 10% PEI, 15% PEI, 20% PEI and 60% PEI, were selected to study the effect of PEI on the crystallization and hydrogen bonding of PVAm / PEI variable stiffness materials, corresponding to PEI mass ratios of 5wt%, 10wt%, 15wt%, 20wt% and 60wt% (the percentage of PEI in the total mass of PVAm and PEI). X-ray diffraction (XRD) analysis of PVAm / PEI variable stiffness materials in dry state ( Figure 2 a) shows a broad amorphous peak at about 25° and a narrower crystalline peak at 33°. The crystallinity of the PVAm / PEI variable stiffness material was calculated ( Figure 2 b), the crystallinity of the pure PVAm film is about 9.41%, which gradually increases with the addition of PEI and then decreases. When the PEI concentration is 15%, the crystallinity of the PVAm / PEI variable stiffness material reaches a maximum value of about 16.55%. This crystallinity shows a downward trend with the further increase of PEI concentration, indicating that the addition of excessive PEI may destroy the crystalline region of PVAm. The addition of PEI increases the intermolecular hydrogen bonding of the system, and strong molecular forces contribute to the orderly arrangement of chain segments, which is conducive to the formation of crystalline regions. However, the addition of excessive PEI may form stronger intermolecular hydrogen bonds, resulting in reduced mobility of the PVAm chain, thereby limiting the crystallization of PVAm. Figure 2 The Fourier transform infrared spectrum in c shows that the -1 The NH stretching vibrations at 2400 and 2600 cm-1 are attributed to the primary amine groups on PVAm. These two v(NH)s are lower than the normal v(NH) range (3300 to 3500 cm-1). -1 ), because of the intramolecular hydrogen bonding of PVAm. When PEI was added to 15wt%, v(NH) became a broad peak ranging from 3200 to 3500cm -1 This is because excess PEI leads to stronger intermolecular hydrogen bonds and destroys the crystallization of PVAm (intramolecular hydrogen bonds), which is consistent with the XRD results.
[0072] The hydrogen bonding association (HBA) of PVAm / PEI in the PVAm / PEI variable stiffness material was determined by calculating the peak area ratio after splitting and fitting ( Figure 2 d). The HBA (intramolecular hydrogen bond) in pure PVAm reaches the highest hydrogen bonding degree (59.11%) because the compound is rich in primary amino groups. However, as the PEI content gradually increases to 10%, the HBA decreases to 547%, at which point intermolecular crosslinks begin to form between PVAm and PEI; as the PEI content reaches 15%, the HBA decreases to 547% at 3200 to 3500 cm -1A broader intermolecular hydrogen bond peak between PVAm and PEI appeared, and intermolecular hydrogen bonds gradually formed. At this time, HBA (intermolecular hydrogen bonds) was about 32.12%, and finally gradually increased to 39% (60% PVAm / PEI). Therefore, when 15% PEI was added to the system, the intermolecular hydrogen bonds were considered to be almost saturated. In addition, the peak at 1660cm -1 The peak in wavenumber is attributed to the NH bending vibration ( Figure 2 e), and with the addition of PEI, the gradual enhancement and red shift of σ(NH) further proves the formation of intermolecular hydrogen bonds. When the PEI content increases from 10% to 15%, HBA increases rapidly from 13.3% to 18.4% and then remains basically unchanged ( Figure 2 f). Therefore, based on XRD and FTIR, it was concluded that the addition of 15 wt% PEI had the highest number of crystallinity and hydrogen bonding.
[0073] Figure 3 The moisture absorption rate of the PVAm / PEI variable stiffness material prepared in the present invention at different relative humidity (RH) The moisture absorption rate of the PVAm / PEI variable stiffness material at 25°C and (a) 25% RH, (b) 55% RH, and (c) 75% RH.
[0074] In order to characterize the humidity absorption rate, the composite film in a dry state was placed in a programmable constant temperature and humidity test box, the temperature was set at 25°C, and the humidity was set at 25% RH, 55% RH and 75% RH, respectively, for humidity absorption test. The composite film in the humidity absorption state showed a trend of "fast first and then slow" ( Figure 3 ), indicating that rapid humidity absorption can be achieved in a relatively short time.
[0075] Figure 4 The stress-strain curves of the PVAm / PEI variable stiffness material prepared in the present invention at 75% RH and different moisture absorption times: (a) 0 minutes, (b) 10 minutes, (c) 20 minutes, (d) 30 minutes, (e) 60 minutes, and (f) 120 minutes.
[0076] According to the stress-strain curves of various variable stiffness material components ( Figure 4), the change of Young's modulus before and after moisture absorption and the range of stiffness change were calculated. The results show that the components of the PVAm / PEI composite film exhibit "rigid and brittle" characteristics in the dry state; the maximum stiffness can reach 1560.85MPa, and the corresponding strain is about 2.9%; after 10 minutes of moisture absorption, water penetrates into the composite film from the surface, destroys the hydrogen bonds between the amine groups, and gradually destroys the crystalline area. The stress of different components of the PVAm / PEI variable stiffness material is reduced by 10 times. However, the presence of water molecules and the main amine groups formed by hydrogen bonds enhance the toughness of the film, increasing its maximum strain by about 3800% relative to the dry state, which is about 1310 times the original, showing the characteristics of "soft and tough". With the increase of moisture absorption time, the stress decreases more slowly. After 120 minutes of moisture absorption, the crystalline area is basically destroyed, and moisture basically replaces the hydrogen bonds between the original amine groups. The stiffness of the 15% PVAm / PEI variable stiffness material before and after moisture absorption was 1560.85MPa and 0.022MPa, respectively, and the stiffness change was about 7.1×10 4 ; See Table 1 for specific results.
[0077] Figure 5 Mechanism characterization of humidity-responsive variable stiffness material obtained in Example 3 of the present invention. (a) XRD of 15% PVAm / PEI variable stiffness material and (b) crystallinity at different moisture absorption times. (c) Changes in transparency of variable stiffness material before and after moisture absorption. (d) In-situ infrared one-dimensional spectrum of 15% PVAm / PEI variable stiffness material at 20-80°C. (d) Measurement of the XRD of 15% PVAm / PEI variable stiffness material at 1750–1500 cm –1 Two-dimensional synchronous infrared correlation spectra of 15% PVAm / PEI variable stiffness materials at different wavenumbers. (e) Two-dimensional correlation spectra of synchronous spectra and (f) asynchronous spectra. (g) Molecular simulation and binding energy calculation of PVAm chains, PEI chains and water molecules.
[0078] according to Figure 5 a, The 15% PVAm / PEI variable stiffness material in the dry state also shows a significantly narrower crystallization peak at 2θ=22° and 33°, and its crystallinity is about 17% ( Figure 5 b). After 5 minutes of moisture absorption, the crystallization peak at 2θ=33° disappeared, and the crystallization area gradually deteriorated. At this time, the crystallinity was about 14.3%. As the moisture absorption time increased, the crystallization peak gradually widened and the crystallinity gradually decreased; after 60 minutes of moisture absorption, the crystal structure was almost destroyed, and the crystallinity dropped to about 6.5%. Due to the moisture absorption process, the crystal area was destroyed, resulting in a decrease in the stiffness of the crystallinity. The transmittance of the variable stiffness material in the dry state was only 30%, and it appeared white and opaque; however, after 180 minutes of moisture absorption, the variable stiffness material became transparent and the transmittance increased to 70%, indicating that the crystallinity had changed ( Figure 5 c). Figure 5d shows the one-dimensional infrared spectrum with an initial temperature of 20 °C and rising to 80 °C. When the temperature is 20 °C, a peak at 3230 cm -1 and 3073cm -1 The double peaks at 1693 cm-1 are attributed to the antisymmetric stretching vibration and symmetric stretching vibration of the main amine groups in PEI and PVAm, respectively. -1 The single peak is attributed to the NH bending vibration of the primary amine group. The formation of hydrogen bonds reduces the bonding constant between hydrogen and nitrogen atoms, resulting in a decrease in the vibration frequency. This is why the curve shows a clear red shift and broadening of the absorption peak as the temperature increases. To further understand the network dynamics of the 15% PEI variable stiffness material during heating, 2D correlation calculations were performed between 20°C and 80°C using the spectral wavenumbers 1750-1500cm -1 The synchronous and asynchronous 2D correlation spectra of the films at wave numbers are shown in Figure 5 e and 5f. Figure 5 Two positive autocorrelation peaks can be seen in e, located at [1688, 1688cm -1 ] and [1556,1556cm -1 ]. These represent the formation of hydrogen-bonded NH moieties and the free NH bending vibration absorption peaks of the primary amine groups. Figure 5 Two positive cross peaks can be observed at the non-diagonal positions of f, located at [1680, 1540 cm -1 ] and [1680,1596cm -1 According to Noda's principle, it can be seen that the first occurrence is at 1680 cm -1 The free NH bond at 1556 cm -1 The NH bonds at the positions of the NH groups change, indicating that the free NH bonds begin to relax first and move to the adjacent hydrogen-bonded chains to form more intermolecular hydrogen bonds. Therefore, the number of intermolecular hydrogen bonds gradually increases, and HBA also rises, which is consistent with the infrared results mentioned above. In addition, molecular dynamics simulations were performed to prove that the hydrogen bonds between the amine groups in the composite film will be replaced by hydrogen bonds between water molecules after moisture absorption ( Figure 5g), COMPASSII force field was used to simulate the molecular dynamics behavior of a composite film mixed with PVAm chains, PEI chains and water molecules before and after moisture absorption. The binding energy of 30 PVAm chains and 10 PEI chains in the composite film is 1448 kcal / mol, while the binding energy between 30 PVAm chains and 1077 water molecules is 4645 kcal / mol, and the binding energy between 30 PEI chains and 540 water molecules is 1788 kcal / mol. The binding energy between PVAm and PEI chains and water molecules is greater than the binding energy between PVAm and PEI chains. This is sufficient to show that the hydrogen bonds between amine groups in the variable stiffness material are replaced by hydrogen bonds after the absorption of water molecules.
[0079] Figure 6 The humidity-responsive variable stiffness material obtained in Example 3 of the present invention is used in intelligent adhesion, shape locking and shape memory. (a) The variable stiffness material is reconfigured into a load-bearing 3D shape; after heating and evaporation of water, the 3D shape is locked; after absorbing moisture, the film can be restored to its original state; (b) The adhesion performance of the variable stiffness material; (c) At 25°C and 75% relative humidity, the angle change of the 15% PVAm / PEI variable stiffness material after different time of moisture absorption.
[0080] PVAm / PEI variable stiffness materials can be used as shape memory and locking materials. The prepared humidity-responsive PVAm / PEI variable stiffness material can be molded into various complex shapes in its soft state, and can be molded into the desired shape by heating; the process is reversible. If the shape needs to be changed, the material can be reshaped by softening by absorbing moisture. The material is universal and can be reshaped into different shapes by absorbing moisture again to meet different needs. The process of absorbing and releasing moisture to change the shape of the same material is as follows Figure 6 a. The soft variable stiffness material can fully replicate the details and lock them in by removing the moisture, even from simple shapes such as squares and triangles to complex five-pointed stars. 4 The shape-locked variable stiffness material can bear a certain external load. Therefore, the variable stiffness material can have a certain load-bearing capacity, shape memory, and can be re-locked into a complex 3D shape due to its two-dimensional scalability. In addition, Figure 6As shown in b, since the stiffness of the variable stiffness material can change quickly and continuously, the hygroscopic material can easily support a weight of approximately 1.7 kg by adhering to a plastic bottle cap and drying quickly. The PVAm / PEI variable stiffness material can quickly change its stiffness, deform in a flexible and controllable manner, and quickly recover its shape memory and lock. The composite shape memory and locking film was placed in a programmable constant temperature and humidity test chamber with a set temperature of 25°C and a humidity of 75% to absorb moisture to examine the shape recovery properties of the variable stiffness material. The change in the recovery angle of the variable stiffness material over time was recorded ( Figure 6 c). In the initial state, the variable stiffness material maintains a shape-locked upright state. When moisture is absorbed for about 100 seconds, the variable stiffness material gradually absorbs moisture and softens. Within 150-160 seconds, the angle of the softened variable stiffness material changes rapidly from 20° to 75°, at which point the variable stiffness material can almost be regarded as restored to the state before shape memory. In other words, the variable stiffness material will basically return to its original state after absorbing moisture for 220 seconds. The study shows that the prepared PVAm / PEI variable stiffness material has timely shape memory and locking properties.
[0081] Table 1. Stiffness properties of PVAm / PEI variable stiffness materials
[0082]
[0083] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A humidity-responsive PVAm / PEI variable stiffness material, characterized in that: The PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 6 to 9.5 parts of polyvinylamine, 0.5 to 4 parts of polyethyleneimine, and 90 parts of water.
2. The PVAm / PEI variable stiffness material according to claim 1, characterized in that: The PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 8 to 9.5 parts of polyvinylamine, 0.5 to 2 parts of polyethyleneimine, and 90 parts of water.
3. The PVAm / PEI variable stiffness material according to claim 1, characterized in that: The PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 8 to 8.5 parts of polyethylene amine, 1.5 to 2 parts of polyethylene imine, and 90 parts of water.
4. The PVAm / PEI variable stiffness material according to claim 1, characterized in that: The PVAm / PEI variable stiffness material is composed of the following raw materials in parts by weight: 8.5 parts of polyvinylamine, 1.5 parts of polyethyleneimine, and 90 parts of water.
5. The PVAm / PEI variable stiffness material according to claim 1, characterized in that: The molecular weight Mw of the polyvinylamine is 1 million to 3 million; the molecular weight Mw of the polyethyleneimine is 10,000 to 50,000.
6. A method for preparing the humidity-responsive PVAm / PEI variable stiffness material according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: Polyethylene amine and polyethylene imine are mixed with water according to the weight ratio to obtain a composite solution, and then the composite solution is poured into a mold, dried, and demolded to obtain a humidity-responsive PVAm / PEI variable stiffness material.
7. The preparation method according to claim 6, characterized in that: The mass percentage of the polyethyleneimine is 5-40%, and the mass percentage of the polyethyleneimine is calculated relative to the sum of the polyethyleneamine and the polyethyleneimine.
8. The preparation method according to claim 6, characterized in that: The drying conditions are 40-60° C., 8-24 h.
9. Application of the PVAm / PEI variable stiffness material according to any one of claims 1 to 5 in smart adhesion, shape locking and shape memory.
10. A PVAm / PEI composite material with shape memory, characterized in that: The PVAm / PEI composite material with shape memory is composed of the following raw materials in parts by weight: 6 to 9.5 parts of polyvinylamine, 0.5 to 4 parts of polyethyleneimine, and 90 parts of water.
Citation Information
Patent Citations
Shape memory polymer variable-stiffness tube and manufacturing method thereof
CN103398240A
Polyvinylamine film with branched network structure as well as preparation method and application of film
CN108816063A
Composite membrane and manufacturing method thereof
KR1020140094853A
Method for manufacturing filler for paper and paper containing same filler for paper manufactured thereby
KR1020150021826A
PROMOTING ENDOTHELIAL CELL AFFINITY AND ANTITHROMBOGENICITY OF POLYTETRAFLUOROETHYLENE (ptfe) BY MUSSEL-INSPIRED MODIFICATION AND RGD / HEPARIN GRAFTING
WO2019232177A1