Lightweight high-thermal-conductivity flame-retardant polyarylene sulfide-based composite material and preparation thereof
By introducing materials such as magnesium oxide whiskers and amino silicone oil into polyaryl sulfide, the problem of combustion risks in new energy vehicles is solved, and a high thermal conductivity and lightweight polyaryl sulfide-based composite material is achieved, which significantly improves the thermal conductivity coefficient. It also reduces density and has good flame retardant properties.
Patent Information
- Application Number
- CN202411187854.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has failed to develop lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composites, especially when used in new energy vehicles for weight reduction and battery protective components, where combustion risks exist.
Magnesium oxide whiskers are used as high thermal conductivity and self-flame retardant enhancement components, combined with polyarylene sulfide containing non-acidic active groups, and lightweight high thermal conductivity self-flame retardant magnesium oxide crystals are prepared through the interface of amino silicone oil and sulfhydryl silicone oil. Polyaryl sulfide functional composite material.
It significantly improves the thermal conductivity, reduces the density by 20-30%, and achieves lightweight effect, and has good flame retardant properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material and a preparation method thereof, and belongs to the field of polymer materials. Background Art
[0002] The rapid development of new energy vehicles represented by lithium batteries has brought with it the demand for lightweight, high thermal conductivity and self-flaming retardant functional materials with better performance as weight-reducing components and battery protection components to avoid battery vehicle combustion, car combustion and other incidents. Among them, polyphenylene sulfide (PPS) is widely used in the automotive field due to its advantages of high temperature resistance, corrosion resistance and high strength. PPS is used in the automotive industry, accounting for about 45%, mainly used for automotive functional parts, igniters, heaters, thermostats, lamp holders, bearings; such as replacing metal to make exhaust pipe circulation valves and water pump impellers, pneumatic signal regulators, etc. With the rise of the use of new energy vehicles, especially the use of lithium batteries, natural and charging combustion may occasionally occur due to battery short circuit, heat accumulation, heating and other reasons, causing casualties and property losses.
[0003] In the prior art, there has been no report on introducing magnesium oxide whiskers into polyarylene sulfide to prepare a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material. Summary of the invention
[0004] In view of the above-mentioned defects, the present invention uses specific magnesium oxide whiskers as high thermal conductivity, self-flame retardant and lightweight reinforcing components, uses polyarylene sulfide containing non-acidic active groups as a matrix, and strengthens the interface with amino silicone oil and mercapto silicone oil to prepare a lightweight, high thermal conductivity, self-flame retardant magnesium oxide whisker polyarylene sulfide functional composite material.
[0005] The technical solution of the present invention:
[0006] The first technical problem to be solved by the present invention is to provide a method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material, the preparation method comprising: firstly mixing modified polyarylene sulfide, magnesium oxide whiskers and a coupling agent; then preparing the polyarylene sulfide-based composite material by melt blending; the mass ratio of the modified polyarylene sulfide to the magnesium oxide whiskers is 50-95:5-50, and the added mass of the coupling agent is 0.5-3.5wt% of the mass of the modified polyarylene sulfide;
[0007] The modified polyarylene sulfide is prepared by the following preparation method: firstly, a sulfur-containing monomer is subjected to a dehydration reaction under the action of an alkali and a polar non-protonic solvent; then monomers M1, M2 and M3 are added to react at 180-280°C for 2-6 hours (after waiting for the formation of oligomers), and then react at 250-300°C for 2-6 hours; then the mixture is cooled to room temperature, and a white product is obtained by washing, filtering and drying, which is the modified polyarylene sulfide; the M1 is a dihalogenated aromatic hydrocarbon, M2 is a dihalogenated aromatic compound having a main chain polar group, and M3 is a dihalogenated aromatic compound having a side chain polar group; the polar group is an alkaline active group.
[0008] Furthermore, the molar amounts of monomers M1, M2 and M3 are recorded as m1, m2 and m3 respectively, m1: (m2 + m3) = 80 ~ 99: 1 ~ 20, m2 and m3 cannot be 0 at the same time; the molar ratio of the sulfur-containing monomer to the monomers M1, M2 and M3 is: sulfur-containing monomer: (m1 + m2 + m3) = 0.95 ~ 1.05: 1.0.
[0009] Furthermore, the polar group is selected from: hydroxyl or amino; preferably amino; the reason why the present invention selects alkaline active groups is that acidic groups such as carboxyl and sulfonic acid groups will react with magnesium oxide, affecting the whisker lattice structure and thus affecting the thermal conductivity of the product.
[0010] Furthermore, the diameter of the magnesium oxide whisker is between 0.2 μm and 1.5 μm, and the aspect ratio is ≥50.
[0011] Furthermore, the coupling agent is selected from amino silicone oil or mercapto silicone oil coupling agent.
[0012] Further, the M1 is a dihalogenated aromatic hydrocarbon, such as at least one of p-dihalobenzene, m-dihalobenzene, naphthalenedihalobenzene or biphenyldihalobenzene;
[0013] M2 is a dihalogenated aromatic compound having a main chain polar group, such as at least one of 4,4'-dihalodiphenyl sulfone, 4,4'-dihalobenzophenone or 4,4'-dihalodiphenyl ether;
[0014] M3 is a dihalogenated aromatic compound having a polar group on the side chain, such as:
[0015] Among them, X=F, Cl, Br.
[0016] Furthermore, the modified polyarylene sulfide is selected from the following substances:
[0017]
[0018] Furthermore, in the above-mentioned method for preparing modified polyarylene sulfide, the drying refers to drying at 80 to 150° C. for 6 to 24 hours.
[0019] Furthermore, the coupling agent is selected from one of the following substances: KH550 (3-aminopropyltriethoxysilane), N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, 3-aminopropyldiethoxymethylsilane, γ-aminoethylaminopropyltrimethoxysilane, silane coupling agent KH-792, KH-580 or KH-540.
[0020] Furthermore, in the above-mentioned method for preparing modified polyarylene sulfide, the sulfur-containing monomer is selected from: sodium sulfide, sodium hydrosulfide or hydrogen sulfide.
[0021] Further, the polar aprotic solvent is selected from: any one of N-methyl-2-pyrrolidone (NMP), N-cyclohexylpyrrolidone (NCHP), 1,3-dimethyl-2-imidazolidinone (DMI), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, 1,3-dimethyl-2-imidazolidinone (MI) lactam, tetramethylurea, dimethyl sulfoxide or sulfolane; the solvent dosage is S 2- (mol) / 0.3-1L.
[0022] Furthermore, the magnesium oxide whisker is prepared by the following preparation method: reacting guanidine carbonate and an aqueous solution of magnesium sulfate heptahydrate or magnesium chloride hexahydrate at room temperature for 1 to 3 hours; then standing and aging for at least 24 hours to obtain a precursor with good crystallization and fibrous appearance; then, stirring and heating to 120°C to 140°C, the pressure is 0.2 to 0.4 MPa, and maintained under this condition for 2 to 5 hours, and then filtered, washed and dried; then the dried magnesium carbonate is further dehydrated, thermally decomposed and cooled to obtain the magnesium oxide whisker; wherein the molar ratio of guanidine carbonate to magnesium sulfate heptahydrate or magnesium chloride hexahydrate is 1 to 2 mol: 1 mol. The Na of the obtained magnesium oxide whisker + The content is less than 30ppm.
[0023] Furthermore, in the above-mentioned method for preparing magnesium oxide whiskers, the washing refers to: washing with deionized water at least 6 times, with the amount of water used each time being 100-200 L; and the drying refers to drying at 80° C. for 10 hours.
[0024] Furthermore, in the above-mentioned method for preparing magnesium oxide whiskers, dehydration and thermal decomposition refer to: transferring the dried magnesium carbonate to a muffle furnace, slowly heating it up at a heating rate of 1 to 5°C / min, maintaining it at 300 to 400°C for 1 to 3 hours, and then heating it to 700 to 800°C and maintaining it for 1 to 5 hours to convert it into magnesium oxide.
[0025] In the present invention, the magnesium oxide whiskers prepared by the method have no residual sodium, potassium and other ions, otherwise lattice defects will occur, causing brittleness, reducing toughness and significantly reducing thermal conductivity; in addition, since the aspect ratio of the precursor is increased by hydration and pressure heat treatment, the aspect ratio of the obtained magnesium oxide whiskers is long, and the larger the crystal, the faster the heat conduction along the crystal surface.
[0026] The second technical problem to be solved by the present invention is to provide a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material, which is prepared by the above-mentioned preparation method.
[0027] The third technical problem to be solved by the present invention is to provide a heat dissipation film, wherein the film is made by using the above-mentioned lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material through the existing film-making method.
[0028] Beneficial effects of the present invention:
[0029] The present invention uses a specific magnesium oxide whisker as a high thermal conductivity, self-flaming retardant and lightweight reinforcing component, uses polyarylene sulfide containing non-acidic active groups as a matrix, and uses amino silicone oil and mercapto silicone oil to strengthen the interface to prepare a lightweight, high thermal conductivity, self-flaming retardant magnesium oxide whisker polyarylene sulfide functional composite material. The thermal conductivity of the obtained composite material can reach 3.6 to 8.6 w / mk, and the thermal conductivity is greatly improved, which is about 50 times higher than that of polyphenylene sulfide, and about 20-30 times higher than that of glass fiber reinforced polyphenylene sulfide; the density is 1.45 to 1.58 g / cm 3 Compared with the current similar polyphenylene sulfide composite materials, its density is reduced by about 20-30%, that is, the lightweight effect is obvious. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material. The preparation method comprises the following steps: firstly, uniformly mixing modified polyarylene sulfide, magnesium oxide whiskers and a coupling agent; and then preparing the polyarylene sulfide-based composite material by melt blending; the mass ratio of the modified polyarylene sulfide to the modified magnesium oxide whiskers is 50-95:5-50, and the added mass of the coupling agent is 0.5-3.5wt% of the mass of the modified polyarylene sulfide;
[0031] Wherein, the structural formula of the modified polyarylene sulfide is shown in Formula I:
[0032] The present invention provides a magnesium oxide whisker / polyarylene sulfide functional composite material, the composition of which is schematically shown as follows:
[0033]
[0034] Specifically:
[0035]
[0036] First, the present invention prepares a magnesium oxide whisker, and the preparation principle and schematic formula are as follows:
[0037]
[0038] Specifically, magnesium oxide whiskers can be prepared by the following method: preparing guanidine carbonate ( The invention discloses a method for preparing a magnesium oxide whisker comprising the steps of: reacting an aqueous solution of magnesium sulfate heptahydrate (MgSO4·7H2O, molecular weight: 121.1) and magnesium sulfate heptahydrate (MgSO4·7H2O, molecular weight: 246.47) or magnesium chloride hexahydrate (MgCl2·6H2O, 203.3) at room temperature (guanidine carbonate: magnesium = 1-2:1 mol); aging the mixture for 24 hours to obtain a precursor basic magnesium sulfate having a well-crystallized and fibrous appearance; drying the mixture at 80°C for 6 hours; heating the mixture (2°C / min) to 750°C and maintaining the mixture for 3 hours; controlling the decomposition rate of the precursor so that the precursor decomposes slowly at low temperature to maintain a whisker-like appearance; and then sintering the mixture at high temperature to obtain magnesium oxide whiskers having a well-sintered, uniformly dispersed and large aspect ratio, wherein the whisker diameter is 0.2μm to 1.5μm and the aspect ratio is ≥50.
[0039] Secondly, the present invention also prepares a polyarylene sulfide containing polar groups that forms an interface bond with magnesium oxide whiskers, which can be prepared in the following manner:
[0040] Since magnesium oxide whiskers have polar and alkaline properties, it is difficult for them to form an interface with polyphenylene sulfide of poor polarity, so it is necessary to modify the structure of polyphenylene sulfide to increase its polarity; however, due to the alkalinity of magnesium oxide whiskers, it is prevented from reacting with acids such as carboxylic acid and sulfonic acid during processing; therefore, it is not suitable to introduce groups such as carboxyl groups and sulfonic acid groups into the structure of polyphenylene sulfide, but it is suitable to introduce groups such as amino groups and hydroxyl groups; accordingly, the structure of the polyarylene sulfide designed by the present invention is:
[0041]
[0042] Among them, m1(mol):(m2+m3)(mol)=80~99:1~20, m2 and m3 cannot be 0 at the same time;
[0043] Y is selected from the following groups: or -O-, etc.; Z is selected from the following groups: benzene ring, polyaromatic ring, etc., as examples; G is hydroxyl -OH or amino -NH2, and preferably hydroxyl;
[0044] Considering the polymer structure composed of m1 (M1), m2 (M2) and m3 (M3), it can be embodied as the following structural formula:
[0045]
[0046] Among M1, M2 and M3, the content (mol) of M1 is greater than or equal to 80%, and the content (mol) of M2+M3 is less than or equal to 20%; wherein, M2 and M3 do not need to exist at the same time, as long as their polarities meet the matching of magnesium oxide whiskers.
[0047] M1 is a dihalogenated aromatic hydrocarbon having the following structure, such as: p-dihalobenzene
[0048] 1-Dihalobenzene Naphthalenedihalobenzenes and biphenyl dihalobenzene wait.
[0049] M2 is a dihalogenated aromatic compound with a main chain polar structure, such as: 4,4'-dihalodiphenyl sulfone 4,4'-Dihalobenzophenone or 4,4'-dihalodiphenyl ether At least one of; wherein, X=F, Cl, Br.
[0050] M3 is a dihalogenated aromatic compound with a polar structure in the side chain, such as: can be the following compounds: dihalogen phenol, such as: dihalogen phenol Dihalonaphthols Dihalogenated polyphenols wait.
[0051] The modified polyarylene sulfide is prepared by the following method: firstly, the sulfur-containing monomer is subjected to a dehydration reaction under the action of an alkali and a polar aprotic solvent; then, M1, M2 and M3 are added to react at 180-280°C for 2-6 hours (after oligomers are formed), and then react at 250-300°C for 2-6 hours; then, the product is cooled to room temperature, washed, filtered and dried to obtain a white product, which is the specific polyarylene sulfide resin. The drying refers to drying at 80-150°C for 6-24 hours; wherein,
[0052] (M1+M2+M3): S 2- (mol) is strictly controlled to be 0.99-1.01:1.00 to ensure that the degree of polymerization of the polymerized polyarylene sulfide is greater than 500.
[0053] The polymerization reaction is shown below:
[0054]
[0055] Furthermore, the ionic sulfur is selected from sodium sulfide, sodium hydrosulfide and hydrogen sulfide.
[0056] Further, the polymerization medium is selected from any one of polar aprotic solvents such as N-methyl-2-pyrrolidone (NMP), N-cyclohexylpyrrolidone (NCHP), 1,3-dimethyl-2-imidazolidinone (DMI), hexamethylphosphoramide (HMPA), N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, 1,3-dimethyl-2-imidazolidinone (MI) lactam, tetramethylurea, dimethyl sulfoxide or sulfolane. The amount of solvent used is S 2- (mol) / 0.3-1L.
[0057] In order to further prepare the magnesium oxide whisker / polyarylene sulfide composite material, due to the organic and inorganic interface problems when the magnesium oxide whisker and the above polyarylene sulfide are compounded, and the polar group content in the sparse polyarylene sulfide is limited, it is necessary to enhance the interface bonding through coupling links. Considering that magnesium oxide whiskers are alkaline, acidic media or groups will cause the whisker structure to be destroyed, and the coupling link can only use a coupling agent with an electron donor structure. The present invention uses the following amino silicone oil or mercapto silicone oil coupling link: KH550 (3-aminopropyltriethoxysilane, ), Si602 (N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane) SI-902(JH-M902)
[0058] 3-Aminopropyldiethoxymethylsilane; γ-aminoethylaminopropyltrimethoxysilane
[0059] Silane coupling agent KH-792 KH-580, 3-Mercaptopropyltriethoxysilane KH-540γ-aminopropyltrimethoxysilane The amount of coupling agent used is (wt%) 0.5-3.5 of the polyarylene sulfide.
[0060] The polyarylene sulfide particles and the magnesium oxide whiskers prepared in the present invention are weighed and mixed according to a specified ratio, and then the coupling agent is added and mixed at high speed in a mixer at a speed of 800-100 rpm for 5-10 minutes.
[0061] Furthermore, the present invention composites magnesium oxide whiskers with polyarylene sulfide: the magnesium oxide whisker polyarylene sulfide mixture with an interface reinforced by amino silicone oil or mercapto silicone oil is dried by vacuum drying at a drying temperature of 80-110° C., and then extruded and granulated by a twin-screw extruder at 310-350° C. to prepare magnesium oxide whisker polyarylene sulfide with different magnesium oxide whisker contents. An injection molding machine is used to injection mold mechanical specimens at 310-350° C. for testing; the magnesium oxide whisker content is measured by burning at 800° C. for 6 hours; and the density is calculated based on weight and volume.
[0062] Furthermore, the composite materials with different magnesium oxide whisker contents are drawn into films through a casting machine as heat dissipation films, and the composite materials containing 2.5-15% (if the whisker content is too high, it cannot be cast into a film and will be brittle. At 2%, the film is transparent, and the light transmittance of the 5% film is worse, but it does not affect the use as a circuit film, etc.) magnesium oxide whisker are drawn into films through a casting machine: the temperature of the first to fourth sections of the screw is 300-350°C, and the speed of the film collecting roller is 10-300mm / min; through the casting process, a cast film with a thickness of 10-250μm is formed, and the thermal conductivity is tested, and it is used as a heat dissipation battery separator or heat dissipation flexible material; the composite material particles containing 10-45% magnesium oxide whiskers are injection molded into a plate (thickness 2-10mm) by an injection molding machine, and the thermal conductivity is measured, and it is used as a solid-state battery packaging separator or heat dissipation plate scenario.
[0063] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.
[0064] Example 1
[0065] 1) Preparation of magnesium oxide whiskers: 12.1 kg of guanidine carbonate was dissolved in 100 L of deionized water, added to a 500 L pressure-lined titanium pressure reactor, and stirred; 24.5 kg of magnesium sulfate heptahydrate was dissolved in 100 L of deionized water, slowly added to the reactor, and the addition was completed within 15 minutes. After stirring for 2 hours, stirring was stopped. After 24 hours, the temperature was raised to 120° C. and the pressure was about 0.2 MPa. The temperature was maintained under this condition for 3 hours (the crystals will grow and the aspect ratio will increase under this condition), and filtered. , washed 6 times with deionized water, each time using 100L of water; then dried at 80°C for 10 hours; then the dried magnesium carbonate was transferred to a muffle furnace, slowly heated at a rate of 2°C / min, kept at 350°C for two hours, and then heated to 750°C for 3 hours (the first stage is the dehydration of the precursor, and then the precursor magnesium carbonate is gradually converted into magnesium oxide during the heating process. The two-stage heating ensures the integrity of the magnesium oxide whisker lattice); naturally cooled to room temperature to obtain 4.0kg of white product; Na + The content is less than 30ppm.
[0066] 2) Preparation of modified polyarylene sulfide: 50 L of NMP, 11.6 kg of sodium hydrosulfide (48%), and 4.0 kg of NaOH were added to a 100 L reactor, heated to 200 ° C under nitrogen protection, and 6.0 L of water was distilled out; then 13.9 kg of p-dichlorobenzene, 2,5-dichlorophenol 0.82kg; react at 220℃ for 3 hours, the first stage reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, wash. Then use deionized water to wash 6 times at 60℃. Then vacuum dry at 120℃ for 24 hours; obtain white particles, i.e. 10.0kg of modified polyarylene sulfide.
[0067] 3) Weigh 0.5 kg of the modified magnesium oxide whisker obtained in step 1) and 4.5 kg of the modified polyarylene sulfide obtained in step 2), add coupling agent KH550 (3-aminopropyltriethoxysilane, ) 130g, mixed at high speed by a mixer, the speed is 900rpm, and the mixing time is 8 minutes;
[0068] 4) The mixed material obtained in step 3) is dried under vacuum at a temperature of 90° C. for 6 hours; then, the mixed material is extruded and granulated at 325° C. using a twin-screw extruder to prepare a magnesium oxide whisker / polyarylene sulfide composite material having a magnesium oxide whisker content of about 10%; mechanical specimens are injection molded at 310-350° C. using an injection molding machine for testing; the magnesium oxide whisker content is measured by burning at 800° C. for 6 hours; and the density is calculated based on weight and volume.
[0069] 5) The magnesium oxide whisker / polyarylene sulfide composite material prepared in step 4) is drawn into a film by a casting machine as a heat dissipation film: the temperatures of the first to fourth sections of the screw are 300, 335, 340, and 335°C, and the speed of the film collecting roller is 100 mm / min; through the casting process, a cast film with a thickness of 100 μm is formed, and the thermal conductivity is tested.
[0070] Performance Testing:
[0071] The obtained composite material particles are injection molded into plates (thickness 2-10mm) by an injection molding machine, and the thermal conductivity is measured for use as solid-state battery packaging partitions or heat sinks.
[0072] The diameter and length of magnesium oxide whiskers were routinely tested using SEN scanning equipment.
[0073] The thermal conductivity is tested according to the national standard of thermal conductivity of ceramic / plastic composite materials.
[0074] Molecular weight and viscosity: expressed by melt index, tested at 315°C and 5kg pressure, the mass in grams flowing out in 10 minutes; g / 10min.
[0075] Film thickness: Labthink CHY-C2A thickness gauge.
[0076] Polarity of polyarylene sulfide - water contact angle: The sample was made into a 2×2 cm film for water contact angle test. The test conditions were: the test temperature was room temperature, the sessile drop method, the drop volume was 2 μL, and six parallel points were measured for each film sample; the statistical analysis software was OriginPro2022b, all data were expressed as mean ± standard deviation, the Kolmogorov-Smirnov method was used for normality test, the Levene method was used for homogeneity of variance test, and the Scheffe test in One Way ANOVA was used for mean comparison.
[0077] Melting point: The DSC test was performed using a DSC 3+ differential scanning calorimeter from Mettler-Toledo, Switzerland. Under a nitrogen atmosphere, the sample was first heated from 40°C to 320°C at a heating rate of 10°C / min, maintained at 320°C for 5 min to eliminate the thermal history, then cooled to 40°C at a cooling rate of 10°C / min, and then heated to 320°C at a heating rate of 10°C / min.
[0078] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ), mass to volume ratio, conventional tests.
[0079] Composite material strength testing: conventional mechanical testing.
[0080] Flame retardant performance: Contact with open flame for 10 seconds, leave, and observe whether it burns during contact with the flame and whether it burns or drips after leaving the flame.
[0081] Test results:
[0082] Magnesium oxide whisker diameter and length: whisker diameter is 0.75±0.25μm, length is 50±25μm;
[0083] Molecular weight and viscosity MI (g / 10min) of polyarylene sulfide: 210 (indicating good processing and film-forming properties);
[0084] Polyarylene sulfide polarity-water contact angle (°): 70;
[0085] Melting point (℃): (1) prepared modified polyarylene sulfide: 285; (2) magnesium oxide whisker / polyarylene sulfide composite material: 289;
[0086] Film thickness (μm): 100±10;
[0087] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0088] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 120; (2) flexural strength (MPa): 160, modulus (GPa): 6;
[0089] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0090] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0091] Example 2 (same as Example 1, except that magnesium sulfate is replaced by magnesium chloride in the preparation of magnesium oxide whisker precursor)
[0092] 1) Preparation of magnesium oxide whiskers: Dissolve 12.1 kg of guanidine carbonate in 100 L of deionized water, add to a 500 L pressurized titanium-lined pressure reactor, and start stirring; dissolve 20.3 kg of magnesium chloride hexahydrate in 100 L of deionized water, slowly add to the reactor, add in 15 minutes, stir for 2 hours and stop stirring, stir and heat to 120 ° C after 24 hours, the pressure is about 0.2 MPa, keep under this condition for three hours, filter, wash with deionized water 6 times, each time using 100 L of water. Then dry at 80 ° C for 10 hours; then transfer the dried magnesium carbonate to a muffle furnace, slowly heat up at a rate of 2 ° C / min, keep at 350 ° C for 2 hours, and then heat to 750 ° C and keep for 3 hours. Naturally cool to room temperature to obtain 4.0 kg of white product. Na + The content is less than 30ppm.
[0093] Steps 2)-5) are the same as in Example 1.
[0094] Test results:
[0095] Magnesium oxide whisker diameter and length: whisker diameter is 0.85±0.25μm, and length is 55±25μm.
[0096] Polyarylene sulfide molecular weight and viscosity MI (g / 10min): 210;
[0097] Polyarylene sulfide polarity-water contact angle (°): 70;
[0098] Melting point (℃): (1) modified polyarylene sulfide: 285; (2) magnesium oxide whisker / polyarylene sulfide composite material: 289;
[0099] Film thickness (μm): 100±10;
[0100] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0101] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 120; (2) flexural strength (MPa): 160, modulus (GPa): 6;
[0102] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0103] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0104] Example 3 (same as Example 1, wherein M2 / M3 are different during the preparation of polyarylene sulfide)
[0105] 1) Same as Example 1.
[0106] 2) Preparation of polyarylene sulfide matched with magnesium oxide whiskers: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.0kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was fractionated, 13.9kg p-dichlorobenzene, 2,5-dichlorohydroquinone were added 0.90kg. React at 220℃ for 3 hours, the first stage reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, and wash. Then use deionized water to wash 6 times at 60℃. Then vacuum dry at 120℃ for 24 hours; obtain 10.0kg of white granular polyarylene sulfide product.
[0107] 3)-5) are the same as in Example 1.
[0108] Test results:
[0109] Diameter and length of magnesium oxide whiskers: whisker diameter is (μm) 0.75±0.25, and length is (μm) 50±25.
[0110] Polyarylene sulfide molecular weight and viscosity (g / 10min): 230;
[0111] Polyarylene sulfide polarity-water contact angle (°): 65;
[0112] Melting point (℃): (1) modified polyarylene sulfide: 287; (2) magnesium oxide whisker / polyarylene sulfide composite material: 292;
[0113] Film thickness (μm): 100±10;
[0114] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0115] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 130; (2) flexural strength (MPa): 180, modulus (GPa): 7;
[0116] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0117] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0118] Example 4 (same as Example 1, wherein M2 / M3 are different during the preparation of polyarylene sulfide)
[0119] 1) Same as Example 1.
[0120] 2) Preparation of polyarylene sulfide matched with magnesium oxide whiskers: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.0kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was fractionated, 13.9kg p-dichlorobenzene, 4,4-dichlorodiphenyl sulfone were added 1.45kg. React at 220℃ for 3 hours, the first stage reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, and wash. Then use deionized water to wash 6 times at 60℃. Then vacuum dry at 120℃ for 24 hours; obtain 10.0kg of white granular polyarylene sulfide product.
[0121] 3)-(5)Same as Example 1.
[0122] Test results:
[0123] Magnesium oxide whisker diameter and length: whisker diameter is (μm) 0.75±0.25, length is (μm) 50±25μm;
[0124] Polyarylene sulfide molecular weight and viscosity (g / 10min): 190;
[0125] Polyarylene sulfide polarity-water contact angle (°): 75;
[0126] Melting point (℃): (1) modified polyarylene sulfide: 284 (2) magnesium oxide whisker / polyarylene sulfide composite material: 287;
[0127] Film thickness (μm): 100±10;
[0128] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0129] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 125; (2) flexural strength (MPa): 170, modulus (GPa): 6.5;
[0130] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0131] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0132] Embodiment 5 (same as embodiment 1, M2 / M3 are different)
[0133] 1) Same as Example 1.
[0134] 2) Preparation of polyarylene sulfide matched with magnesium oxide whiskers: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.0kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was fractionated, 13.2kg p-dichlorobenzene, 2,5-dichlorophenol were added 0.82kg, 4,4-dichlorodiphenyl sulfone 1.45kg. React at 220℃ for 3 hours, the first stage reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, and wash. Then use deionized water to wash 6 times at 60℃. Then vacuum dry at 120℃ for 24 hours; obtain 10.2kg of white granular polyarylene sulfide product.
[0135] 3)-(5)Same as Example 1.
[0136] Test results:
[0137] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.80±0.3, length (μm) 50±25μm;
[0138] Polyarylene sulfide molecular weight and viscosity (g / 10min): 260;
[0139] Polyarylene sulfide polarity-water contact angle (°): 62;
[0140] Melting point (℃): (1) modified polyarylene sulfide: 283 (2) magnesium oxide whisker / polyarylene sulfide composite material: 286;
[0141] Film thickness (μm): 100±10;
[0142] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0143] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 122; (2) flexural strength (MPa): 168, modulus (GPa): 6;
[0144] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0145] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0146] Example 6 (same as Example 1, different M2 / M3 contents)
[0147] 1) Same as Example 1
[0148] 2) Preparation of polyarylene sulfide matched with magnesium oxide whiskers: 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.0kg NaOH were added to a 100L reactor, heated to 200°C under nitrogen protection, 6.0L water was fractionated, 13.2kg p-dichlorobenzene, 2,5-dichlorophenol were added 1.6kg. React at 220℃ for 3 hours, the first stage reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, and wash. Then use deionized water to wash 6 times at 60℃. Then vacuum dry at 120℃ for 24 hours; obtain 10.0kg of white granular polyarylene sulfide product.
[0149] 3)-(5)Same as Example 1.
[0150] Test results:
[0151] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.75±0.25, length (μm) 50±25;
[0152] Polyarylene sulfide molecular weight and viscosity (g / 10min): 210;
[0153] Polyarylene sulfide polarity-water contact angle (°): 60;
[0154] Melting point (℃): (1) modified polyarylene sulfide: 288 (2) magnesium oxide whisker / polyarylene sulfide composite material: 293;
[0155] Film thickness (μm): 100±10;
[0156] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0157] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 119; (2) flexural strength (MPa): 163, modulus (GPa): 6;
[0158] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0159] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0160] Example 7 (same as Example 1, but with a different magnesium oxide whisker content of about 20%)
[0161] 1)-2) Same as Example 1;
[0162] 3) Weigh 1.0 kg of magnesium oxide whiskers obtained in step 1) and 4.0 kg of polyarylene sulfide obtained in step 2), add coupling agent KH550 (3-aminopropyltriethoxysilane, )110g, mixed with a mixer at high speed, the rotation speed is 900rpm, and the mixing time is 8 minutes.
[0163] 4)-5) Same as Example 1.
[0164] Test results:
[0165] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.75±25, length (μm) 50±25;
[0166] Polyarylene sulfide molecular weight and viscosity (g / 10min): 210;
[0167] Polyarylene sulfide polarity-water contact angle (°): 70;
[0168] Melting point (℃): (1) modified polyarylene sulfide: 285; (2) magnesium oxide whisker / polyarylene sulfide composite material: 292;
[0169] Injection molding plate thickness (mm): 5±0.5.
[0170] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.52;
[0171] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 150; (2) flexural strength (MPa): 180, modulus (GPa): 7;
[0172] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 6.8;
[0173] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0174] Example 8 (same as Example 1, but with a different magnesium oxide whisker content of about 40%)
[0175] 1)-2) Same as Example 1;
[0176] 3) Weigh 2.0 kg of magnesium oxide whiskers obtained in step 1) and 3.0 kg of polyarylene sulfide obtained in step 2), add coupling agent KH550 (3-aminopropyltriethoxysilane, )100g; mixed by a mixer at high speed, the speed is 900rpm, and the mixing time is 8 minutes.
[0177] 4)-5) Same as Example 1.
[0178] Test results:
[0179] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.75±25, length (μm) 50±25;
[0180] Polyarylene sulfide molecular weight and viscosity (g / 10min): 210;
[0181] Polyarylene sulfide polarity-water contact angle (°): 58;
[0182] Melting point (℃): (1) Modified polyarylene sulfide: 285 (2) MgO whisker / polyarylene sulfide composite material: 293
[0183] Injection molding plate thickness (mm): 5±0.5;
[0184] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.58;
[0185] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 180; (2) flexural strength (MPa): 220, modulus (GPa): 9.8;
[0186] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 8.6;
[0187] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0188] Example 9 (same as Example 1, different coupling agent)
[0189] 1)-2) Same as Example 1.
[0190] 3) Weigh 0.5 kg of magnesium oxide whiskers obtained in step 1) and 4.5 kg of polyarylene sulfide obtained in step 2), add coupling agent KH-540 (γ-aminopropyltrimethoxysilane )130g, through the high-speed mixing machine, the rotation speed is 900rpm, the mixing time is 10 minutes.
[0191] 4)-5) Same as Example 1.
[0192] Test results:
[0193] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.75±25, length (μm) 50±25μm;
[0194] Polyarylene sulfide molecular weight and viscosity (g / 10min): 210;
[0195] Polyarylene sulfide polarity-water contact angle (°): 70;
[0196] Melting point (℃): (1) Modified polyarylene sulfide: 285 (2) MgO whisker / polyarylene sulfide composite material: 289
[0197] Film thickness (μm): 100±10;
[0198] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0199] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 125; (2) flexural strength (MPa): 170, modulus (GPa): 6.5;
[0200] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0201] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0202] Example 10 (same as Example 1, but with different coupling agent content).
[0203] 1)-2) Same as Example 1.
[0204] 3) Weigh 0.5 kg of magnesium oxide whiskers obtained in (1) and 4.5 kg of polyarylene sulfide obtained in (2), add coupling agent KH550 (3-aminopropyltriethoxysilane, )150g, mixed with a mixer at high speed, the rotation speed is 900rpm, and the mixing time is 8 minutes.
[0205] 4)-5) Same as Example 1
[0206] Test results:
[0207] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.75±25, length (μm) 50±25;
[0208] Polyarylene sulfide molecular weight and viscosity (g / 10min): 210;
[0209] Polyarylene sulfide polarity-water contact angle (°): 70;
[0210] Melting point (℃): (1) modified polyarylene sulfide: 285; (2) magnesium oxide whisker / polyarylene sulfide composite material: 289;
[0211] Film thickness (μm): 100±10;
[0212] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3):1.45;
[0213] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 128; (2) flexural strength (MPa): 175, modulus (GPa): 6.5;
[0214] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.6;
[0215] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
[0216] Comparative Example 1 Compared with Traditional Polyphenylene Sulfide
[0217] Add 50L NMP, 11.6kg sodium hydrosulfide (48%), 4.0kg NaOH into a 100L reactor, heat to 200℃ under nitrogen protection, distill out 6.0L water, add 14.7kg p-dichlorobenzene. React at 220℃ for 3 hours, and the first stage of reaction is completed; heat to 260℃ for 3 hours, cool to 150℃, slowly add deionized water, filter, and wash. Then use deionized water to wash 6 times at 60℃. Then vacuum dry at 120℃ for 24 hours; obtain 10.0kg of white granular polyarylene sulfide product.
[0218] Test results:
[0219] Polyarylene sulfide molecular weight and viscosity (g / 10min): 520;
[0220] Polyarylene sulfide polarity-water contact angle (°): 108;
[0221] Melting point (℃): (1) polyphenylene sulfide: 285;
[0222] Film thickness (μm): Difficult to draw the film;
[0223] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 70; (2) flexural strength (MPa): 95, modulus (GPa): 3.9;
[0224] Thermal conductivity of aromatic sulfide composite material (w / mk): 0.2;
[0225] Flame retardant properties of polyphenylene sulfide: extinguishes when away from fire and does not drip.
[0226] Comparative Example 2 (Using Traditional Polyphenylene Sulfide and Magnesium Oxide Micron Powder)
[0227] 4.5 kg of polyphenylene sulfide prepared in Comparative Example 1 and 0.5 kg of magnesium oxide micron powder (magnesium oxide micron powder is purchased from Aladdin reagent, irregular spherical powder) were mixed and extruded into granules at 320° C.; film drawing and injection molding were performed;
[0228] Polyarylene sulfide polarity-water contact angle (°): 108;
[0229] Melting point (℃): (1) polyphenylene sulfide: 285 (2) magnesium oxide whisker / polyphenylene sulfide composite material: 287;
[0230] Film thickness (μm): 100±10;
[0231] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0232] Mechanical strength test of magnesium oxide powder / polyarylene sulfide composite material: (1) tensile strength (MPa): 110; (2) flexural strength (MPa): 145, modulus (GPa): 5.5;
[0233] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 1.5;
[0234] Flame retardant properties of magnesium oxide powder / polyarylene sulfide composite materials: non-flammable;
[0235] The mechanical properties and thermal conductivity are 20-50% worse than those of the embodiment.
[0236] Comparative Example 3 (using the polyarylene sulfide of Example 1 and conventional magnesium oxide micron powder)
[0237] The rest is the same as in Example 1, except that the magnesium oxide whiskers in Example 1 are replaced with conventional magnesium oxide micron powder.
[0238] Test results: Melting point (℃): (1) Modified polyarylene sulfide: 285 (2) MgO whisker / polyarylene sulfide composite material: 287;
[0239] Film thickness (μm): 100±10;
[0240] Density of magnesium oxide (powder) / polyarylene sulfide composite material (g / cm 3 ):1.45;
[0241] Mechanical strength test of magnesium oxide powder / polyarylene sulfide composite material: (1) tensile strength (MPa): 115; (2) flexural strength (MPa): 150, modulus (GPa): 4.9;
[0242] Thermal conductivity of magnesium oxide powder / polyarylene sulfide composite material (w / mk): 1.6;
[0243] Flame retardant properties of magnesium oxide powder / polyarylene sulfide composite materials: non-flammable;
[0244] The mechanical properties and thermal conductivity are 20-50% worse than those of the embodiment.
[0245] Comparative Example 4, same as Example 1, without using coupling agent
[0246] Test results:
[0247] Magnesium oxide whisker diameter and length: whisker diameter (μm) 0.75±25, length (μm) 50±25μm;
[0248] Polyarylene sulfide molecular weight and viscosity (g / 10min): 210;
[0249] Polyarylene sulfide polarity-water contact angle (°): 70;
[0250] Melting point (℃): (1) polymer: 285; (2) magnesium oxide whisker / polyarylene sulfide composite material: 288;
[0251] Film thickness (μm): 100±10;
[0252] Density of magnesium oxide / polyarylene sulfide composites (g / cm 3 ):1.45;
[0253] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 110; (2) flexural strength (MPa): 145, modulus (GPa): 4.9;
[0254] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 2.9;
[0255] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable;
[0256] The mechanical properties are 10-20% worse than those of Example 1.
[0257] Comparative Example 5 (MgO micron powder content is 40%)
[0258] Same as in Comparative Example 2, the content of magnesium oxide micron powder was increased to 40% (ie, the mass ratio of magnesium oxide powder to the sum of magnesium oxide powder and polyphenylene sulfide).
[0259] Test results:
[0260] Polyarylene sulfide molecular weight and viscosity (g / 10min): 510;
[0261] Polyarylene sulfide polarity-water contact angle (°): 10;
[0262] Melting point (℃): (1) modified polyarylene sulfide: 285; (2) magnesium oxide powder / polyarylene sulfide composite material: 287;
[0263] Injection molding plate thickness (mm): 5±0.5;
[0264] Density of magnesium oxide powder / polyarylene sulfide composite material (g / cm 3 ):1.65;
[0265] Mechanical strength test of magnesium oxide whisker / polyarylene sulfide composite material: (1) tensile strength (MPa): 100; (2) flexural strength (MPa): 10, modulus (GPa): 7;
[0266] Thermal conductivity of magnesium oxide / polyarylene sulfide composite material (w / mk): 3.9;
[0267] Flame retardant properties of magnesium oxide whisker / polyarylene sulfide composite materials: non-flammable.
Claims
1. A method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material, characterized in that: The preparation method comprises: firstly mixing the modified polyarylene sulfide, magnesium oxide whisker and coupling agent; then preparing the polyarylene sulfide-based composite material by melt blending; the mass ratio of the modified polyarylene sulfide to the magnesium oxide whisker is 50-95:5-50, and the added mass of the coupling agent is 0.5-3.5wt% of the mass of the modified polyarylene sulfide; The modified polyarylene sulfide is prepared by the following preparation method: firstly, a sulfur-containing monomer is subjected to a dehydration reaction under the action of an alkali and a polar non-protonic solvent; then, monomers M1, M2 and M3 are added and reacted at 180 to 280°C for 2 to 6 hours, and then at 250 to 300°C for 2 to 6 hours; then, the mixture is cooled to room temperature, and a white product is obtained by washing, filtering and drying, which is the modified polyarylene sulfide; the M1 is a dihalogenated aromatic hydrocarbon, the M2 is a dihalogenated aromatic compound having a main chain polar group, and the M3 is a dihalogenated aromatic compound having a polar group on the side chain, and the polar group is an alkaline active group.
2. The method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to claim 1, characterized in that: The molar amounts of the monomers M1, M2 and M3 are recorded as m1, m2 and m3 respectively, m1: (m2 + m3) = 80-99: 1-20, and m2 and m3 cannot be 0 at the same time; the molar ratio of the sulfur-containing monomer to the monomers M1, M2 and M3 is: sulfur-containing monomer: (m1 + m2 + m3) = 0.95-1.05: 1.0; The polar group is selected from: hydroxyl or amino; preferably amino.
3. The method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to claim 1 or 2, characterized in that: The diameter of the magnesium oxide whisker is 0.2 μm to 1.5 μm, and the aspect ratio is ≥50; Further, the coupling agent is selected from amino silicone oil or mercapto silicone oil coupling agent; Furthermore, the coupling agent is selected from one of the following substances: 3-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, 3-aminopropyldiethoxymethylsilane, γ-aminoethylaminopropyltrimethoxysilane, silane coupling agent KH-792, KH-580 or KH-540.
4. A method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to any one of claims 1 to 3, characterized in that: The M1 is selected from at least one of p-dihalobenzene, m-dihalobenzene, naphthalenedihalobenzene or biphenyldihalobenzene; The M2 is selected from at least one of 4,4'-dihalodiphenyl sulfone, 4,4'-dihalodiphenyl ketone or 4,4'-dihalodiphenyl ether; The M3 is selected from: Among them, X=F, Cl, Br.
5. The method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to any one of claims 1 to 4, characterized in that: The modified polyarylene sulfide is selected from the following structures: Among them, m1:(m2+m3)=80~99:1~20, m2 and m3 cannot be 0 at the same time.
6. A method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to any one of claims 1 to 5, characterized in that: The sulfur-containing monomer is selected from: sodium sulfide, sodium hydrosulfide or hydrogen sulfide.
7. A method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to any one of claims 1 to 6, wherein the polar aprotic solvent is selected from: N-methyl-2-pyrrolidone, N-cyclohexylpyrrolidone, 1,3-dimethyl-2-imidazolidinone, hexamethylphosphoramide, N,N-dimethylacetamide, N,N-dimethylamide, N-ethylcaprolactam, N,N-vinylpyrrolidone, 1,3-dimethyl-2-imidazolidinone (MI) lactam, tetramethyl urea, dimethyl sulfoxide or cyclopentane sulfone.
8. A method for preparing a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material according to any one of claims 1 to 7, characterized in that: The magnesium oxide whisker is prepared by the following preparation method: reacting guanidine carbonate and an aqueous solution of magnesium sulfate heptahydrate or magnesium chloride hexahydrate at room temperature for 1 to 3 hours; then standing and aging for at least 24 hours to obtain a precursor; then stirring and heating to 120° C. to 140° C., a pressure of 0.2 to 0.4 MPa, maintaining under this condition for 2 to 5 hours, and then filtering, washing and drying; then further dehydrating, thermally decomposing and cooling the dried magnesium carbonate to obtain the magnesium oxide whisker; wherein the molar ratio of guanidine carbonate to magnesium sulfate heptahydrate or magnesium chloride hexahydrate is 1 to 2:1; Furthermore, the Na + Content less than 30ppm; Furthermore, in the preparation method of the magnesium oxide whisker, dehydration and thermal decomposition refer to: transferring the dried magnesium carbonate to a heating device, slowly heating it up at a rate of 1 to 5°C / min, maintaining it at 300 to 400°C for 1 to 3 hours, and then heating it to 700 to 800°C and maintaining it for 1 to 5 hours.
9. A lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material, characterized in that: The composite material is prepared by the preparation method according to any one of claims 1 to 8.
10. A heat dissipation film, characterized in that: The film is made of a lightweight, highly thermally conductive, flame-retardant polyarylene sulfide-based composite material as described in claim 9.
Citation Information
Cited By
High-flame-retardant lightweight flame-retardant material and preparation method thereof
CN120424500A