Antibacterial and mildew-proof shaving board and preparation method thereof
Through the combination of nano zinc oxide modified phenolic resin and lignin modified mugwort fiber, the existing antibacterial and anti-mold particleboard has been solved, with the problem of insufficient effect, complex process and high cost, and the durable anti-bacterial and anti-mold effect and good effect are achieved The physical and mechanical properties meet the environmental protection needs of the construction and furniture industries.
Patent Information
- Application Number
- CN202411272010.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing antibacterial and anti-mold particleboard has not lasting effect, the preparation process is complex and costly, and some antibacterial agents have potential harm to the human body and the environment, making it difficult to meet the demand for environmentally friendly materials in the modern construction and furniture industries.
The nano-zinc oxide modified phenolic resin and lignin-modified wormwood fiber were combined. The antibacterial properties of nano-zinc oxide and photocatalytic effects, the natural antibacterial components of wormwood fibers and the bonding properties of phenolic resins were prepared. Antibacterial and anti-mold particle board, combined with the antibacterial properties of lignin and the modification of silane coupling agent, form a long-lasting anti-bacterial and anti-mold effect and maintain good physical and mechanical properties.
It realizes the durability and mechanical properties of antibacterial and anti-mold effect, simplifies the preparation process, reduces costs, and improves environmental protection, so that particleboard effectively inhibits the growth of mold and bacteria under various environmental conditions, satisfying the construction and furniture. industry demand.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of particle boards, and in particular to an antibacterial and mildew-proof particle board and a preparation method thereof. Background Art
[0002] With the rapid development of modern construction and furniture industry, the requirements for material performance are increasing day by day, especially in terms of antibacterial and mildew resistance. During the use of traditional particleboard, due to the influence of environmental humidity, temperature and other factors, it is easy to breed mold and bacteria, which not only affects the appearance and service life of the product, but also may pose a potential threat to human health.
[0003] At present, there are many kinds of antibacterial and mildew-proof particle boards on the market, but most of them have the following problems: first, the antibacterial and mildew-proof effect is not long-lasting, and the antibacterial performance gradually weakens over time; second, the preparation process is complicated and the cost is high, which is not conducive to large-scale production; third, some antibacterial agents have potential hazards to the human body or the environment and do not meet environmental protection requirements.
[0004] In view of the above problems, it is urgent to develop a particleboard with long-lasting antibacterial and mildew-proof effects, simple preparation process, low cost and environmental protection. The particleboard should be able to effectively inhibit the growth of mold and bacteria under various environmental conditions, while maintaining good physical and mechanical properties to meet the needs of the construction and furniture industries.
[0005] Based on this, the present invention proposes an antibacterial and mildew-proof particle board and a preparation method thereof. Summary of the invention
[0006] The present invention provides an antibacterial and mildew-proof particleboard and a preparation method thereof, wherein the prepared particleboard has a long-lasting antibacterial and mildew-proof effect, a simple preparation process, low cost and is environmentally friendly. The particleboard should be able to effectively inhibit the growth of mold and bacteria under various environmental conditions while maintaining good physical and mechanical properties to meet the needs of the construction and furniture industries.
[0007] The technical solution of the present invention is as follows: In a first aspect, the present invention provides an antibacterial and mildew-proof particleboard, comprising the following raw materials in parts by weight: 15-20 parts of wood particles, 5-6 parts of lignin-modified wormwood fibers, and 2-2.4 parts of modified phenolic resin adhesive.
[0008] As a further technical solution, the shavings are wood shavings, specifically including at least one of poplar, pine and oak; the shavings have a length of 10-12 mm, a width of 5-6 mm and a thickness of 0.2-0.3 mm.
[0009] As a further technical solution, the preparation method of the lignin-modified wormwood fiber includes: mixing the pretreated wormwood fiber with ethanol, adding purified lignin and a silane coupling agent and mixing evenly at a temperature of 45-55°C, a stirring speed of 200-220r / min, a stirring time of 35-45min, and after the stirring is completed, washing and drying to obtain the lignin-modified plant fiber.
[0010] As a further technical solution, the weight ratio of the pretreated wormwood fiber, ethanol, purified lignin and silane coupling agent is (12-14): (70-80): (2.5-3.5): (1.2-1.4).
[0011] As a further technical solution, the preparation method of the pretreated wormwood fiber includes: washing the wormwood, drying it at 60-70°C to remove impurities, and mechanically crushing it into 1-3mm wormwood fiber; impregnating the wormwood fiber in a sodium hydroxide solution with a mass concentration of 9%-10% for 20-24 minutes at a temperature of 60-70°C, and then washing and drying to obtain the pretreated wormwood fiber.
[0012] As a further technical solution, the preparation method of purified lignin includes: gradually adding lignin to a sodium hydroxide aqueous solution, stirring until the lignin is completely dissolved, then standing at room temperature for 20-24 hours, filtering to remove insoluble matter, and obtaining a black lignin solution; adjusting the solution pH to 2.0 with hydrochloric acid, precipitating lignin, and obtaining purified lignin through centrifugation, acid washing, and freeze drying.
[0013] As a further technical solution, the mass fraction of the sodium hydroxide aqueous solution is 2%-3%; the dosage ratio of the sodium hydroxide aqueous solution to lignin is (90-100) mL: (7-8) g.
[0014] As a further technical solution, the modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and its preparation method includes: stirring the phenolic resin at a speed of 400-500r / min, then slowly adding nano zinc oxide and continuing to stir for 30-40min, and ultrasonically treating the stirred mixture for 2-3h; the addition amount of the nano zinc oxide is 3%-5% of the phenolic resin.
[0015] As a further technical solution, the solid content of the phenolic resin is 40% and the pH is 10.5.
[0016] In a second aspect, the present invention proposes a method for preparing an antibacterial and mildew-proof particleboard, the steps comprising: preparing lignin-modified wormwood fiber and a modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and the modified phenolic resin adhesive, performing a first hot pressing at a temperature of 120-130°C for 25-35 minutes; performing a second hot pressing at a temperature of 90-100°C for 50-60 minutes; the hot pressing pressure is 1.5-2.5MPa; after cooling, standing at room temperature for 5-6 days, keeping the moisture content of the particleboard not more than 4%, and trimming and sanding the hot-pressed blank.
[0017] The working principle and beneficial effects of the present invention are: 1. When the particleboard is prepared by compounding nano zinc oxide modified phenolic resin and lignin modified wormwood fiber in the present invention, the durability of the antibacterial and mildew-proof effect and the maintenance of mechanical properties are achieved through the antibacterial property and photocatalytic effect of nano zinc oxide, the natural antibacterial components of wormwood fiber and the bonding property and mechanical properties of phenolic resin. Among them, phenolic resin, as a traditional adhesive, has good bonding properties and mechanical properties. In the particleboard preparation process, phenolic resin can firmly bond lignin modified wormwood fiber together to form a board with certain strength and rigidity. The addition of nano zinc oxide not only improves the antibacterial property of phenolic resin, but also may enhance its mechanical properties to a certain extent. The small size effect and surface effect of nanoparticles enable them to fill the micropores and defects in the resin matrix, improving the density and strength of the matrix. At the same time, chemical bonds or physical entanglements may be formed between nano zinc oxide and the resin matrix, further enhancing the interfacial bonding force between the resin and the fiber. As the main skeleton material of particleboard, the mechanical properties and durability of lignin-modified wormwood fiber have an important influence on the overall mechanical properties of the board. Lignin modification improves the strength and toughness of the fiber, allowing the fiber to better withstand and disperse stress when subjected to external forces.
[0018] 2. The present invention uses lignin-modified wormwood fiber as the raw material of particleboard, which can not only significantly improve the antibacterial and mildew-proof properties of particleboard, but also maintain its good physical and mechanical properties, and at the same time realize the simplification of preparation process, cost control and environmental protection. Lignin itself has certain antibacterial properties, and its complex chemical structure can destroy the cell wall of bacteria or molds and inhibit their growth. Through the purification process, the antibacterial components of lignin are further concentrated, which enhances its antibacterial effect. Wormwood itself contains a variety of active ingredients with antibacterial and mildew-proof effects, such as volatile oils, flavonoids, etc. Combining wormwood fiber with lignin, the two produce a synergistic effect in antibacterial and mildew-proofing, so that the modified wormwood fiber has stronger antibacterial and mildew-proofing capabilities. And the two are combined through the modification of silane coupling agent, and the silane coupling agent forms a protective film on the fiber surface, which not only improves the water resistance of the fiber, but also enhances the stability of the antibacterial and mildew-proof components, making the antibacterial and mildew-proof effect more durable.
[0019] 3. The lignin-modified wormwood fiber prepared in the present invention has certain strength and toughness. After being modified by lignin and silane coupling agent, the bonding force between the fibers is enhanced, thereby improving the physical and mechanical properties of the particleboard. The protective film and cross-linked structure formed by lignin and silane coupling agent on the fiber surface help maintain the structural stability of the particleboard during use and prevent deformation or cracking caused by factors such as environmental humidity and temperature changes. In addition, wormwood is a widely distributed plant among the raw materials used, with abundant resources and easy to obtain. Lignin is a by-product of industries such as pulping and papermaking, and also has high availability. As raw materials, wormwood and lignin have relatively low costs, which helps to reduce the overall production cost of particleboard. And lignin-modified wormwood fiber as a raw material for particleboard makes particleboard easy to degrade after being abandoned, and will not cause long-term burden on the environment.
[0020] 4. Phenolic resin is used as a particleboard adhesive. Nano zinc oxide is used to modify it in the present invention. Nano zinc oxide exhibits excellent antibacterial properties due to its extremely small particle size and high specific surface area. There are a large number of oxygen vacancies and zinc ions on its surface, which can destroy the cell walls and cell membranes of bacteria or molds, inhibiting their growth and reproduction. In addition, nano zinc oxide can also produce a photocatalytic effect under light, further killing or inhibiting the growth of microorganisms. Nano zinc oxide is evenly dispersed in phenolic resin, and stirring and ultrasonic treatment are used to ensure that the nanoparticles form a good combination with the resin matrix. This combination not only improves the stability of nano zinc oxide, but also enables the antibacterial and mildew-proof components to be evenly distributed inside the particleboard, thereby achieving a lasting antibacterial and mildew-proof effect. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The phenolic resin in the present invention is purchased from Guangdong Taier Adhesive Co., Ltd.; the silane coupling agent is KH570.
[0023] Example 1 The present embodiment provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood chips, 5.5 parts of lignin-modified wormwood fibers, and 2.2 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the length of the wood chips is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; In other embodiments, waterproof, flame retardant, mildew-proof, and sterilization additives may also be added.
[0024] Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 65°C to remove impurities, and mechanically crushed to produce 2 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 9.5% for 22 minutes at a temperature of 65°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 2.5% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 22 hours, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze drying; the ratio of sodium hydroxide aqueous solution to lignin is 95 mL:7.5 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 50°C, with a stirring speed of 210 r / min; the stirring time was 40 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 13:75:3:1.3; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 450 r / min, then slowly adding nano zinc oxide and continuing stirring for 35 minutes, and ultrasonically treating the stirred mixture for 2.5 hours; the amount of nano zinc oxide added is 4% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, standing at room temperature for 5.5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0025] Example 2 The present embodiment provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 15 parts of wood chips, 5 parts of lignin-modified wormwood fibers, and 2 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the wood chips are 10 mm long, 5 mm wide, and 0.2 mm thick; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 60°C to remove impurities, and mechanically crushed to produce 1 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 9% for 20 minutes at a temperature of 60°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 2% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 20 h, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze-drying; the ratio of sodium hydroxide aqueous solution to lignin is 90 mL:7 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 45°C and a stirring speed of 200 r / min; the stirring time was 35 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 12:70:2.5:1.2; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 400 r / min, then slowly adding nano zinc oxide and continuing stirring for 30 minutes, and ultrasonically treating the stirred mixture for 2 hours; the amount of nano zinc oxide added is 3% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 120° C. for 25 minutes; performing a second hot pressing at a temperature of 90° C. for 50 minutes; the hot pressing pressure is 1.5 MPa; after cooling, standing at room temperature for 5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0026] Example 3 The present embodiment provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 20 parts of wood chips, 6 parts of lignin-modified wormwood fibers, and 2.4 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the length of the wood chips is 12 mm, the width is 6 mm, and the thickness is 0.3 mm; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 70°C to remove impurities, and mechanically crushed to produce 3 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 10% for 24 minutes at a temperature of 70°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 3% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 24 hours, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze-drying; the ratio of sodium hydroxide aqueous solution to lignin is 100 mL: 8 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 55°C and a stirring speed of 220 r / min; the stirring time was 45 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 14:80:3.5:1.4; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 500 r / min, then slowly adding nano zinc oxide and continuing stirring for 40 minutes, and ultrasonically treating the stirred mixture for 3 hours; the amount of nano zinc oxide added is 5% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 130° C. for 35 minutes; performing a second hot pressing at a temperature of 100° C. for 60 minutes; the hot pressing pressure is 2.5 MPa; after cooling, standing at room temperature for 6 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0027] Example 4 The present embodiment provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 20 parts of wood chips, 5 parts of lignin-modified wormwood fibers, and 2.4 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the length of the wood chips is 10 mm, the width is 6 mm, and the thickness is 0.2 mm; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 70°C to remove impurities, and mechanically crushed to produce 1 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 10% for 20 minutes at a temperature of 70°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 2% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 24 h, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze-drying; the ratio of sodium hydroxide aqueous solution to lignin is 90 mL: 8 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 45°C, with a stirring speed of 220 r / min; the stirring time was 35 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 14:70:3.5:1.2; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 500 r / min, then slowly adding nano zinc oxide and continuing stirring for 30 minutes, and ultrasonically treating the stirred mixture for 3 hours; the amount of nano zinc oxide added is 3% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 130° C. for 25 minutes; performing a second hot pressing at a temperature of 100° C. for 50 minutes; the hot pressing pressure is 2.5 MPa; after cooling, standing at room temperature for 5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the particle board.
[0028] Comparative Example 1 The present comparative example provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood chips, 5.5 parts of lignin-modified wormwood fibers, and 2.2 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the length of the wood chips is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 65°C to remove impurities, and mechanically crushed to produce 2 mm mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 2.5% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 22 hours, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze drying; the ratio of sodium hydroxide aqueous solution to lignin is 95 mL:7.5 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 50°C, with a stirring speed of 210 r / min; the stirring time was 40 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 13:75:3:1.3; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 450 r / min, then slowly adding nano zinc oxide and continuing stirring for 35 minutes, and ultrasonically treating the stirred mixture for 2.5 hours; the amount of nano zinc oxide added is 4% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, standing at room temperature for 5.5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0029] Comparative Example 2 The present comparative example provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood chips, 5.5 parts of lignin-modified wormwood fibers, and 2.2 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the length of the wood chips is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 65°C to remove impurities, and mechanically crushed to produce 2 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 9.5% for 22 minutes at a temperature of 65°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and lignin and silane coupling agent were added and mixed evenly at a temperature of 50°C, and the stirring speed was 210 r / min; the stirring time was 40 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, lignin and silane coupling agent was 13:75:3:1.3; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 450 r / min, then slowly adding nano zinc oxide and continuing stirring for 35 minutes, and ultrasonically treating the stirred mixture for 2.5 hours; the amount of nano zinc oxide added is 4% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, standing at room temperature for 5.5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0030] Comparative Example 3 The present comparative example provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood chips, 5.5 parts of wormwood fiber, and 2.2 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar; the length of the wood chips is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; The preparation method of wormwood fiber includes: washing wormwood, drying at 65°C to remove impurities, and mechanically crushing to obtain 2mm wormwood fiber; soaking the wormwood fiber in a sodium hydroxide solution with a mass concentration of 9.5% for 22 minutes at a soaking temperature of 65°C, and then washing and drying to obtain the wormwood fiber; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 450 r / min, then slowly adding nano zinc oxide and continuing stirring for 35 minutes, and ultrasonically treating the stirred mixture for 2.5 hours; the amount of nano zinc oxide added is 4% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, standing at room temperature for 5.5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0031] Comparative Example 4 The present comparative example provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood chips, 5.5 parts of lignin-modified wormwood fibers, and 2.2 parts of modified phenolic resin adhesive; the wood chips are wood chips, specifically poplar wood; the length of the wood chips is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 65°C to remove impurities, and mechanically crushed to produce 2 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 9.5% for 22 minutes at a temperature of 65°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 2.5% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 22 hours, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze drying; the ratio of sodium hydroxide aqueous solution to lignin is 95 mL:7.5 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 50°C, with a stirring speed of 210 r / min; the stirring time was 40 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 13:75:3:1.3; The modified phenolic resin adhesive is a nano-titanium dioxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 450 r / min, then slowly adding nano-titanium dioxide and continuing stirring for 35 minutes, and ultrasonically treating the stirred mixture for 2.5 hours; the amount of nano-titanium dioxide added is 4% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and modified phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, standing at room temperature for 5.5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0032] Comparative Example 5 In this comparative example, an antibacterial and mildew-proof particleboard is provided, which is composed of the following raw materials in parts by weight: 17 parts of wood particles, 5.5 parts of lignin-modified wormwood fibers, and 2.2 parts of phenolic resin adhesive; the wood particles are wood particles, specifically poplar wood; the length of the wood particles is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; Among them, the preparation method of lignin modified wormwood fiber includes: (1) Preparation of pretreated mugwort fiber: The mugwort was washed, dried at 65°C to remove impurities, and mechanically crushed to produce 2 mm mugwort fiber; the mugwort fiber was immersed in a sodium hydroxide solution with a mass concentration of 9.5% for 22 minutes at a temperature of 65°C, and then washed and dried to obtain the pretreated mugwort fiber; (2) Preparation of purified lignin: gradually add lignin to a 2.5% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 22 hours, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze drying; the ratio of sodium hydroxide aqueous solution to lignin is 95 mL:7.5 g; (3) Preparation of lignin-modified mugwort fiber: The pretreated mugwort fiber was mixed with ethanol, and purified lignin and silane coupling agent were added and mixed evenly at a temperature of 50°C, with a stirring speed of 210 r / min; the stirring time was 40 min. After the stirring was completed, the fiber was washed and dried to obtain lignin-modified plant fiber; the weight ratio of the pretreated mugwort fiber, ethanol, purified lignin and silane coupling agent was 13:75:3:1.3; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing lignin-modified wormwood fiber and phenolic resin adhesive, stirring and mixing the wood chips, lignin-modified wormwood fiber and phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2 MPa; after cooling, standing at room temperature for 5.5 days, maintaining the moisture content of the particle board at 4%, trimming and sanding the hot-pressed blank to obtain the obtained board.
[0033] Comparative Example 6 The present comparative example provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood particles, 2.2 parts of lignin-modified phenolic resin adhesive; the wood particles are wood particles, specifically poplar wood; the length of the wood particles is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; Among them, the preparation method of the lignin modified phenolic resin adhesive includes: (1) Preparation of purified lignin: gradually add lignin to a 2.5% sodium hydroxide aqueous solution, stir until the lignin is completely dissolved, then let stand at room temperature for 22 h, filter to remove insoluble matter, and obtain a black lignin solution; adjust the solution pH to 2.0 with hydrochloric acid to precipitate lignin, and obtain purified lignin after centrifugation, acid washing, and freeze-drying; the ratio of sodium hydroxide aqueous solution to lignin is 95 mL:7.5 g; (2) Preparation of lignin-modified phenolic resin adhesive: Phenolic resin and ethanol were mixed, purified lignin and silane coupling agent were added, and the mixture was uniformly mixed at a temperature of 50°C and a stirring speed of 210 r / min. The stirring time was 40 min. After the stirring was completed, the mixture was washed and dried to obtain lignin-modified plant fiber. The weight ratio of phenolic resin, ethanol, purified lignin and silane coupling agent was 13:75:3:1.3. The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing a lignin-modified phenolic resin adhesive, stirring and mixing the wood particles and the lignin-modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, the particle board is allowed to stand at room temperature for 5.5 days, the moisture content of the particle board is maintained at 4%, and the hot-pressed blank is trimmed and sanded to obtain the obtained board.
[0034] Comparative Example 7 The present comparative example provides an antibacterial and mildew-proof particleboard, which is composed of the following raw materials in parts by weight: 17 parts of wood particles, 2.2 parts of modified phenolic resin adhesive; the wood particles are wood particles, specifically poplar wood; the length of the wood particles is 11 mm, the width is 5.5 mm, and the thickness is 0.25 mm; The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and the preparation method thereof comprises: stirring the phenolic resin at a speed of 450 r / min, then slowly adding nano zinc oxide and continuing stirring for 35 min, and ultrasonically treating the stirred mixture for 2.5 h; the amount of nano zinc oxide added is 4% of the phenolic resin; the solid content of the phenolic resin is 40%, and the pH is 10.5; The preparation method of the antibacterial and mildew-proof particle board comprises the following steps: preparing a modified phenolic resin adhesive, stirring and mixing the wood particles and the modified phenolic resin adhesive, performing a first hot pressing at a temperature of 125° C. for 30 minutes; performing a second hot pressing at a temperature of 95° C. for 55 minutes; the hot pressing pressure is 2MPa; after cooling, the particle board is allowed to stand at room temperature for 5.5 days, the moisture content of the particle board is maintained at 4%, and the hot pressed blank is trimmed and sanded to obtain the obtained board.
[0035] Test Example 1: The antibacterial and mildew-proof particleboards prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-7, with a thickness of 10 mm, were subjected to the following tests: Mechanical properties: The mechanical properties of particleboard were tested according to GB / T4897-2015 "Particleboard" standard; Antibacterial performance: The oscillation method of GB / T 20944.3-2008 was used, and Escherichia coli, Staphylococcus aureus and Candida albicans were selected as the test bacteria. Five samples of each embodiment and comparative example were tested in parallel, and the average value was taken. Antibacterial effect evaluation: the antibacterial rate of Escherichia coli and Staphylococcus aureus was ≥70%, and the antibacterial rate of Candida albicans was ≥60%, which indicated that the test bacteria had an antibacterial effect. The results are shown in Table 1 below: Table 1
[0036] The present invention simulates a high temperature and high humidity environment. The high temperature environment is placed at 35° C. for 30 days, and the high humidity environment is placed at a humidity of 50% for 30 days. At this time, the internal bonding strength of the particleboard in Example 1 is still maintained at 0.64 MPa and 0.62 MPa; the antibacterial rate is also maintained at 96%-97% after being placed in the two environments for 30 days.
[0037] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An antibacterial and mildew-proof particleboard, characterized in that: The invention comprises the following raw materials in parts by weight: 15-20 parts of wood chips, 5-6 parts of lignin-modified wormwood fibers, and 2-2.4 parts of modified phenolic resin adhesive.
2. The antibacterial and mildew-proof particle board according to claim 1, characterized in that: The wood shavings are wood shavings, specifically including at least one of poplar, pine and oak.
3. The antibacterial and mildew-proof particle board according to claim 1, characterized in that: The preparation method of the lignin modified wormwood fiber comprises: mixing the pretreated wormwood fiber with ethanol, adding purified lignin and a silane coupling agent, mixing evenly at a temperature of 45-55° C., stirring at a speed of 200-220 r / min, stirring for 35-45 min, and after stirring, washing and drying to obtain the lignin modified plant fiber.
4. The antibacterial and mildew-proof particle board according to claim 3, characterized in that: The weight ratio of the pretreated wormwood fiber, ethanol, purified lignin and silane coupling agent is (12-14): (70-80): (2.5-3.5): (1.2-1.4).
5. The antibacterial and mildew-proof particle board according to claim 3, characterized in that: The preparation method of the pretreated wormwood fiber comprises: washing the wormwood, drying at 60-70° C. to remove impurities, and mechanically crushing the wormwood to prepare 1-3 mm wormwood fibers; soaking the wormwood fibers in a sodium hydroxide solution with a mass concentration of 9%-10% for 20-24 minutes at a soaking temperature of 60-70° C., and then washing and drying to obtain the pretreated wormwood fibers.
6. The antibacterial and mildew-proof particle board according to claim 3, characterized in that: The preparation method of the purified lignin comprises: gradually adding lignin to a sodium hydroxide aqueous solution, stirring until the lignin is completely dissolved, then standing at room temperature for 20-24 hours, filtering to remove insoluble matter, and obtaining a black lignin solution; adjusting the solution pH to 2.0 with hydrochloric acid, precipitating lignin, and obtaining purified lignin through centrifugation, acid washing, and freeze drying.
7. The antibacterial and mildew-proof particle board according to claim 6, characterized in that: The mass fraction of the sodium hydroxide aqueous solution is 2%-3%; the dosage ratio of the sodium hydroxide aqueous solution to lignin is (90-100) mL: (7-8) g.
8. The antibacterial and mildew-proof particle board according to claim 1, characterized in that: The modified phenolic resin adhesive is a nano zinc oxide modified phenolic resin, and its preparation method comprises: stirring the phenolic resin at a speed of 400-500 r / min, then slowly adding nano zinc oxide and continuing stirring for 30-40 minutes, and ultrasonically treating the stirred mixture for 2-3 hours; the addition amount of the nano zinc oxide is 3%-5% of the phenolic resin.
9. The antibacterial and mildew-proof particle board according to claim 8, characterized in that: The solid content of the phenolic resin is 40%, and the pH value is 10.
5.
10. A method for preparing the antibacterial and mildew-proof particleboard according to any one of claims 1 to 9, characterized in that the steps include: The lignin-modified wormwood fiber and the modified phenolic resin adhesive are prepared. The wood chips, the lignin-modified wormwood fiber and the modified phenolic resin adhesive are stirred and mixed, and the first hot pressing is performed at a temperature of 120-130° C. for 25-35 minutes; the second hot pressing is performed at a temperature of 90-100° C. for 50-60 minutes; the hot pressing pressure is 1.5-2.5 MPa; after cooling, the wood chips are allowed to stand at room temperature for 5-6 days, the moisture content of the particleboard is kept not more than 4%, and the hot-pressed blank is trimmed and sanded to obtain the obtained board.
Citation Information
Cited By
Biological functional veneer artificial board containing herbal active substances
CN120116299A
Antibacterial and mildew-proof shaving board and preparation method thereof
CN121374783A