Preparation method of phosphate tinting pigment iron magnesium oxide inorganic coating

The preparation of iron-magnesium oxide powder by mixing grinding and calcining treatment in anhydrous ethanol has solved the application limitations of iron-magnesium oxide in the phosphate system, and achieved low-cost, large-scale production and good stability of phosphoric acid Salt-colored pigment, with good matching and corrosion resistance, is suitable for coating applications.

CN118931248APending Publication Date: 2024-11-12SHENYANG INSTITUTE OF CHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410962990.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The application of existing iron and magnesium oxides in catalysis, energy storage and environmental restoration is limited by high cost, potential toxicity and limited availability, and it is difficult to produce large-scale and add phosphate systems to successfully color, affecting the uniformity and stability of the coating. sex.

Method used

The ratio of magnesium oxide and iron oxide to mix and grind in anhydrous ethanol with a molar mass ratio of 1:0.84~1.16. After suction filtration, tableting and calcination treatment, a ferromagnesium oxide powder was formed, with an addition amount of 0.1-3%. When matched with the phosphate coating, the color remains uniform and does not fade after curing at 300-500℃.

Benefits of technology

It realizes mass production with low cost and simple operation, reduces energy consumption, is green and environmentally friendly, and has no pollution. The raw materials have little impact on the phosphate system, have good stability and no anti-corrosion effect. The coating has good coloring and corrosion resistance. Strong alkali resistance and adhesion ability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a phosphate tinting pigment iron-magnesium oxide inorganic coating, and relates to a preparation method of an inorganic coating, and the iron-magnesium oxide comprises the following components: magnesium oxide and iron oxide according to a molar mass ratio of 1: (0.84-1.16). The specific operation comprises the following steps: sampling according to the proportion, grinding, tabletting, calcining at 1100-1400 DEG C, preserving heat for 2-10 hours to obtain a dark purple brown product, grinding, and sieving with a 100-mesh sieve to obtain a final product. The preparation of the coloring pigment iron-magnesium oxide in the phosphate inorganic coating has the characteristics of low cost, simplicity in operation, mass production and the like, and the prepared iron-magnesium oxide has the characteristics of good matching property with the phosphate coating, high coloring power and no fading after high-temperature sintering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an inorganic coating, in particular to a method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating. Background Art

[0002] Fe2MgO4 is a composite oxide and a spinel oxide that has been pursued for its potential applications due to its unique properties and structure. Fe2MgO4 has been widely studied for its potential applications in catalysis, energy storage, and environmental remediation. In catalysis, Fe2MgO4 exhibits excellent catalytic activity in some reactions, such as the oxidation of carbon monoxide and the reduction of nitrogen monoxide. In energy storage, Fe2MgO4 has been studied as a potential electrode material for lithium-ion batteries due to its high theoretical capacity and excellent cycling stability. In environmental remediation, Fe2MgO4 has been studied for its ability to remove pollutants from water and air. Fe2MgO4 has several advantages in laboratory experiments, including its stability, ease of synthesis, and potential use in a wide range of applications. However, there are also some limitations to its use, including its high cost, potential toxicity, and limited availability. There are several methods for synthesizing Fe2MgO4, including solid-state reaction, coprecipitation, sol-gel and hydrothermal synthesis. Solid-state reaction involves mixing precursor materials in a high-temperature furnace, resulting in the formation of Fe2MgO4. Coprecipitation involves precipitating metal ions from a solution, which is then formed through a series of chemical reactions. The sol-gel method involves the formation of a gel-like material, which is then dried and calcined to produce Fe2MgO4. Hydrothermal synthesis involves the reaction of metal precursors in a high-pressure, high-temperature environment to produce Fe2MgO4. Therefore, reducing costs, simplifying operations, and achieving mass production are the efforts of all researchers, and the perfect addition of the obtained Fe2MgO4 to the phosphate system and successful coloring have become the current research content and difficulties of the coating. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating. The method has the characteristics of simple operation and mass production. When the coloring pigment is added in an amount of 0.1-3%, it has good matching with the phosphate coating. After curing at 300-500°C, the coating has uniform color and does not fade.

[0004] The technical solution of the present invention is: A method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating, the method comprising the following preparation steps: (1) Weighing magnesium oxide and iron oxide in a molar mass ratio of 1:(0.84-1.16), mixing and grinding in a ball mill using anhydrous ethanol as a grinding aid to obtain a mixture; (2) Filter the resulting mixture and dry it in a ventilated place; (3) The dried product is pressed into tablets and calcined in a furnace at 1100-1400°C in an air atmosphere; (4) Keep warm at this temperature for 2 to 10 hours; (5) When the temperature in the furnace drops to room temperature, take out the finished product and grind it into powder and pass it through a 100-mesh sieve; (6) The application of iron magnesium oxide as a coloring pigment in phosphate inorganic coatings. When the addition amount is 0.1-3%, it has good matching with the phosphate coating, and after curing at 300-500℃, the coating has uniform color.

[0005] The method for preparing a phosphate coloring pigment iron-magnesium oxide inorganic coating comprises a coloring pigment iron-magnesium oxide in the phosphate inorganic coating, and the magnesium oxide is 1-20 μm.

[0006] The method for preparing a phosphate coloring pigment iron-magnesium oxide inorganic coating comprises a coloring pigment iron-magnesium oxide in the phosphate inorganic coating, and the iron oxide is 1-20 μm.

[0007] The method for preparing a phosphate coloring pigment iron-magnesium oxide inorganic coating comprises an industrial-grade anhydrous ethanol as the coloring pigment iron-magnesium oxide in the phosphate inorganic coating.

[0008] The advantages and beneficial effects of the present invention are: 1. The present invention has the characteristics of low cost, simple operation and mass production.

[0009] 2. The coloring pigment provided by the present invention can reduce energy consumption, is green and environmentally friendly, does not pollute the environment, and is harmless.

[0010] 3. The residual amount of raw materials in the present invention has little effect on the phosphate system, has excellent stability and does not affect the anti-corrosion effect of the original coating.

[0011] 4. When the addition amount of the finished product prepared by the present invention is 0.1-3%, it has good matching property with the phosphate coating. After being cured at 300-500°C, the coating has uniform color and does not fade.

[0012] The invention is different from other coloring pigments. After being cured at 300-500°C, the coating has uniform color and does not fade. As a colorant of the coating, it ensures that the coating has good coloring effect, corrosion resistance, alkali resistance, strong adhesion, and close combination of the coating and the substrate.

[0013] The coloring pigment iron-magnesium oxide in the phosphate inorganic coating of the present invention is made of magnesium oxide and iron oxide with low cost, and has the characteristics of simple operation and mass production. When the addition amount is 0.1-3%, it has good matching with the phosphate coating, and after curing at 300-500°C, the coating has uniform color and does not fade. It does not contain impurities such as other catalysts, and there are few residual substances that affect the phosphate system, so that the coating maintains stability and does not affect the anti-corrosion effect of the original coating. DETAILED DESCRIPTION

[0014] The present invention is further described in detail below by way of examples. Example 1

[0015] In this embodiment, the preparation method of the coloring pigment iron magnesium oxide in the phosphate inorganic coating is as follows: 1. Weigh magnesium oxide and iron oxide in a molar mass ratio of 1:0.92, and grind them in a ball mill with anhydrous ethanol as a grinding aid to obtain a mixture: 2. Filter the obtained mixture and dry it in a ventilated place; 3. The dried product is pressed into tablets and calcined in a furnace at 1250°C in an air atmosphere; 4. Keep warm for 3 hours at this temperature; 5. When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve for standby use.

[0016] The prepared iron magnesium oxide powder is taken out, and it can be observed that the product is dark purple-brown. When it is added into the phosphate system, bubbles are observed to be generated. The comprehensive amount of raw materials can be used to determine the excess magnesium oxide powder, which affects the stability of the coating in the final product. Example 2

[0017] In this embodiment, the preparation method of the coloring pigment iron magnesium oxide in the phosphate inorganic coating is as follows: 1. Weigh magnesium oxide and iron oxide in a molar mass ratio of 1:1.08, and grind them in a ball mill with anhydrous ethanol as a grinding aid to obtain a mixture: 2. Filter the obtained mixture and dry it in a ventilated place; 3. The dried product is pressed into tablets and calcined in a furnace at 1250°C in an air atmosphere; 4. Keep warm for 3 hours at this temperature; 5. When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve for standby use.

[0018] The prepared iron-magnesium oxide powder is taken out, and it can be observed that the product is dark brown. When it is added into the phosphate system, bubbles are observed to be generated. The amount of raw materials used can be combined to determine the excess iron oxide powder, which affects the stability of the coating in the final product. Example 3

[0019] In this embodiment, the preparation method of the coloring pigment iron magnesium oxide in the phosphate inorganic coating is as follows: 1. Weigh magnesium oxide and iron oxide in a molar mass ratio of 1:1, and grind them in a ball mill with anhydrous ethanol as a grinding aid to obtain a mixture: 2. Filter the obtained mixture and dry it in a ventilated place; 3. The dried product is pressed into tablets and calcined in a furnace at 1250°C in an air atmosphere; 4. Keep warm for 3 hours at this temperature; 5. When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve for standby use.

[0020] The prepared iron magnesium oxide powder is taken out, and it can be observed that the product is dark purple-brown. When it is added into the phosphate system, it can be observed that almost no bubbles are generated. When the addition amount is 0.1-3%, it has a good match with the phosphate coating. After curing at 300-500℃, the coating has uniform color, and the advantages of corrosion resistance, alkali resistance, strong adhesion, and close bonding between the coating and the substrate still exist. Example 4

[0021] In this embodiment, the preparation method of the coloring pigment iron magnesium oxide in the phosphate inorganic coating is as follows: 1. Weigh magnesium oxide and iron oxide in a molar mass ratio of 1:1, and grind them in a ball mill with anhydrous ethanol as a grinding aid to obtain a mixture: 2. Filter the obtained mixture and dry it in a ventilated place; 3. The dried product is pressed into tablets and calcined in a furnace at 1250°C in an air atmosphere; 4. Keep warm at this temperature for 5 hours; 5. When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve for standby use.

[0022] The prepared iron magnesium oxide powder is taken out, and it can be observed that the product is dark purple-brown. When it is added into the phosphate system, it can be observed that almost no bubbles are generated. When the addition amount is 0.1-3%, it has a good match with the phosphate coating. After curing at 300-500℃, the coating has uniform color, and the advantages of corrosion resistance, alkali resistance, strong adhesion, and close bonding between the coating and the substrate still exist. Example 5

[0023] In this embodiment, the preparation method of the coloring pigment iron magnesium oxide in the phosphate inorganic coating is as follows: 1. Weigh magnesium oxide and iron oxide in a molar mass ratio of 1:1, and grind them in a ball mill with anhydrous ethanol as a grinding aid to obtain a mixture: 2. Filter the obtained mixture and dry it in a ventilated place; 3. The dried product is pressed into tablets and calcined in a furnace at 1100°C in an air atmosphere; 4. Keep warm for 3 hours at this temperature; 5. When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve for standby use.

[0024] The prepared iron-magnesium oxide powder was taken out and the product was observed to be light purple-brown. When it was added to the phosphate system, bubbles were observed to be generated. It was inferred that the remaining unreacted Fe2O3, MgO, Mg, Fe x O y or Fe x Mg y O z Etc. The final product is not suitable for phosphate system coloring and stable storage. Example 6

[0025] In this embodiment, the preparation method of the coloring pigment iron magnesium oxide in the phosphate inorganic coating is as follows: 1. Weigh magnesium oxide and iron oxide in a molar mass ratio of 1:1, and grind them in a ball mill with anhydrous ethanol as a grinding aid to obtain a mixture: 2. Filter the obtained mixture and dry it in a ventilated place; 3. The dried product is pressed into tablets and calcined in a furnace at 1250°C in an air atmosphere; 4. Keep warm at this temperature for 10 hours; 5. When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve for standby use.

[0026] The prepared iron magnesium oxide powder is taken out, and it can be observed that the product is dark purple-brown. When it is added into the phosphate system, it can be observed that almost no bubbles are generated. When the addition amount is 0.1-3%, it has a good match with the phosphate coating. After curing at 300-500℃, the coating has uniform color, and the advantages of corrosion resistance, alkali resistance, strong adhesion, and close bonding between the coating and the substrate still exist.

Claims

1. A method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating, characterized in that: The method comprises the following preparation steps: (1) Weighing magnesium oxide and iron oxide in a molar mass ratio of 1:(0.84-1.16), mixing and grinding in a ball mill using anhydrous ethanol as a grinding aid to obtain a mixture; (2) Filter the resulting mixture and dry it in a ventilated place; (3) The dried product is pressed into tablets and calcined in a furnace at 1100-1400°C in an air atmosphere; (4) Keep warm at this temperature for 2 to 10 hours; (5) When the temperature in the furnace drops to room temperature, take out the finished product, grind it into powder and pass it through a 100-mesh sieve; (6) The application of iron magnesium oxide as a coloring pigment in phosphate inorganic coatings. When the addition amount is 0.1-3%, it has good matching with the phosphate coating, and after curing at 300-500℃, the coating has uniform color.

2. The method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating according to claim 1, characterized in that: The coloring pigment in the phosphate inorganic coating is iron-magnesium oxide, and the size of the magnesium oxide is 1-20 μm.

3. The method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating according to claim 1, characterized in that: The coloring pigment in the phosphate inorganic coating is iron-magnesium oxide, and the iron oxide has a size of 1-20 μm.

4. The method for preparing a phosphate coloring pigment iron magnesium oxide inorganic coating according to claim 1, characterized in that: The iron-magnesium oxide coloring pigment in the phosphate inorganic coating uses industrial-grade anhydrous ethanol.