Hydrophobic coating for aluminum alloy wheel and preparation method of hydrophobic coating

Through multi-layer hydrophobic coating structure and electrostatic spraying technology, the problem of insufficient density of acrylic resin coating on the surface of aluminum alloy wheels is solved, and efficient anti-fouling and corrosion resistance and easy cleaning are achieved, which improves the added value of wheel coating. .

CN118931311APending Publication Date: 2024-11-12CITIC DICASTAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411030267.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The acrylic resin coating used on the surface of existing aluminum alloy wheels lacks density, which affects the anti-fouling and corrosion effect of the coating.

Method used

Using a multi-layer hydrophobic coating structure consisting of epoxy resin, polyester resin, transparent paint and fluoro-silicon system additive, including primer coating, primer coating, color paint coating and HFC functional coating, through The electrostatic spraying technology deposits and cures in sequence to form a hydrophobic effect with a surface water drop angle greater than 95°.

Benefits of technology

It significantly improves the pollution resistance and easy cleaning of the aluminum alloy wheel surface, enhances the added value of the coating, and meets the needs of efficient pollution and corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931311A_ABST
    Figure CN118931311A_ABST
Patent Text Reader

Abstract

The invention relates to a hydrophobic coating for an aluminum alloy wheel and a preparation method of the hydrophobic coating, and belongs to the technical field of automobile hub manufacturing, the hydrophobic coating for the aluminum alloy wheel comprises a bottom powder coating, a primer coating, a colored paint coating and an HFC functional coating which are sequentially stacked from inside to outside by taking the aluminum alloy wheel as a substrate; the HFC functional coating further comprises transparent paint and an auxiliary agent added into the transparent paint, resin contained in the transparent paint is at least one of acrylic resin, alkyd resin, phenolic resin and polyester resin, and the auxiliary agent is a fluorine and silicon system. The hydrophobic coating for the aluminum alloy wheel not only can meet all paint film tests of the existing aluminum alloy wheel, but also can achieve an obvious hydrophobic effect, the anti-pollution capacity of the surface of a hub is improved, cleaning is easy, and the coating additional value of the hub is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile wheel hub manufacturing, and in particular to a hydrophobic coating for an aluminum alloy wheel and a preparation method thereof. Background Art

[0002] Hydrophobic coatings have unique surface functions such as self-cleaning, high anti-fouling and hydrophobic oil displacement. Using this coating on the surface of different devices can prevent or reduce the adhesion of water vapor, ice and snow and other pollutants, and has important application value in the automotive, aviation and aerospace fields. The use scenarios of automobile wheels are complex and demanding. The coating used on the surface of well-known aluminum alloy wheels is an acrylic resin system, but the acrylic resin system lacks density and has a relatively large surface energy, which seriously affects the anti-fouling and anti-corrosion effect of the coating.

[0003] Therefore, in view of the problems existing in the prior art, the designers of this case actively studied and improved the hydrophobic coating for aluminum alloy wheels and the preparation method thereof. Summary of the invention

[0004] The first purpose of the present invention is to provide a hydrophobic coating for aluminum alloy wheels in view of the defects in the prior art that the coating used on the surface of aluminum alloy wheels is an acrylic resin system, but the acrylic resin system lacks density and has a relatively large surface energy, which seriously affects the anti-fouling and anti-corrosion effects of the coating.

[0005] The second purpose of the present invention is to provide a method for preparing a hydrophobic coating for aluminum alloy wheels in view of the defects in the prior art that the coating used on the surface of the aluminum alloy wheel is an acrylic resin system, but the acrylic resin system lacks density and has a relatively large surface energy, which seriously affects the anti-fouling and anti-corrosion effects of the coating.

[0006] To achieve the first object of the present invention, the present invention provides a hydrophobic coating for an aluminum alloy wheel, the hydrophobic coating for an aluminum alloy wheel comprising: a primer coating, a primer coating, a color paint coating, and an HFC functional coating which are sequentially stacked from the inside to the outside with the aluminum alloy wheel as a substrate, wherein:

[0007] The base powder coating further comprises a base powder resin, a curing agent, a pigment filler and an auxiliary agent, wherein the base powder resin is a dual system of epoxy resin and polyester resin, wherein the epoxy resin and the polyester resin are curing agents for each other, the pigment filler is barium sulfate and carbon black, and the auxiliary agent is a leveling agent, a breathable agent, a brightener and a hardener;

[0008] The primer coating further comprises a primer resin, a dispersant, a pigment filler, a cosolvent, water, a wetting and leveling agent, a defoamer, an additive and a thickener, and the primer resin is an epoxy resin system;

[0009] The paint coating further comprises paint resin, solvent, filler, and additives, wherein the filler is aluminum powder and pigment;

[0010] The HFC functional coating further comprises a transparent paint and an auxiliary agent added to the transparent paint, the resin contained in the transparent paint is at least one of acrylic resin, alkyd resin, phenolic resin and polyester resin, and the auxiliary agent is a fluorine-plus-silicon system.

[0011] Optionally, the water drop angle on the surface of the hydrophobic coating for the aluminum alloy wheel is greater than 95°.

[0012] Optionally, the hydrophobic coating surface for aluminum alloy wheels has a water drop angle of 97.8°.

[0013] Optionally, the primer coating has a thickness of 80 to 120 μm.

[0014] Optionally, the total thickness of the primer coating and the color paint coating is 30 to 60 μm.

[0015] Optionally, the HFC functional coating has a thickness of 15 to 30 μm.

[0016] To achieve the second object of the present invention, the present invention provides a method for preparing a hydrophobic coating for an aluminum alloy wheel, the method for preparing a hydrophobic coating for an aluminum alloy wheel comprising:

[0017] Executing step S1: pre-treating the surface of the aluminum alloy wheel without chromium;

[0018] Executing step S2: depositing a primer coating, a primer coating, and a color paint coating on the surface of the aluminum alloy wheel in sequence by electrostatic spraying, and performing a curing process;

[0019] Execute step S3: deposit the HFC functional coating on the outer surface of the color paint coating by electrostatic spraying.

[0020] Optionally, in step S2, an electrostatic spraying method is used to deposit a primer coating on the surface of the aluminum alloy wheel, and the process parameters are: powder spraying amount 60-70 g / min, voltage 45-70 KV, static electricity 45-60 μA, total gas volume 4.5-5 MPa, baking temperature 160-200°C, and baking time 10-30 min.

[0021] Optionally, the primer coating and the color paint coating are deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the process parameters are: baking temperature 140-160° C., and baking time 10-30 minutes.

[0022] Optionally, an HFC functional coating is deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the process parameters are: baking temperature 140-160° C., and baking time 10-30 min.

[0023] Optionally, the HFC functional coating is prepared by using a transparent lacquer and adding an auxiliary agent to the transparent lacquer and stirring, the auxiliary agent ratio is 0.3% to 1%, the stirring speed is 1000 r / min, and the stirring time is 10 to 15 min.

[0024] In summary, the hydrophobic coating for aluminum alloy wheels of the present invention can not only meet all paint film tests of existing aluminum alloy wheels, but also achieve obvious hydrophobic effect, improve the anti-fouling ability of the wheel hub surface, be easy to clean, and increase the added value of wheel hub coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Shown is a schematic diagram of the hydrophobic coating structure for aluminum alloy wheels of the present invention;

[0026] Figure 2 Shown is a flow chart of a method for preparing a hydrophobic coating for an aluminum alloy wheel according to the present invention;

[0027] Figure 3 Shown is a water drop angle detection spectrum of the hydrophobic coating surface used for aluminum alloy wheels of the present invention. DETAILED DESCRIPTION

[0028] In order to explain the technical content, structural features, objectives and effects of the present invention in detail, the following will be described in detail with reference to embodiments and accompanying drawings.

[0029] See also Figure 1 , Figure 1 The hydrophobic coating for aluminum alloy wheels of the present invention is shown as a schematic diagram. The hydrophobic coating for aluminum alloy wheels comprises: a base powder coating 11, a primer coating 12, a color paint coating 13, and an HFC functional coating 14 are sequentially stacked from the inside to the outside, with the aluminum alloy wheel 10 as a substrate, wherein:

[0030] The base powder coating 11 further includes a base powder resin, a curing agent, a pigment filler and an auxiliary agent, wherein the base powder resin is a dual system of epoxy resin and polyester resin, wherein the epoxy resin and the polyester resin are curing agents for each other, the pigment filler is barium sulfate and carbon black, and the auxiliary agent is a leveling agent, a breathable agent, a brightener and a hardener;

[0031] The primer coating 12 further comprises a primer resin, a dispersant, a pigment filler, a cosolvent, water, a wetting and leveling agent, a defoamer, an additive and a thickener, and the primer resin is an epoxy resin system;

[0032] The paint coating 13 further includes paint resin, solvent, filler, and additives, wherein the filler is aluminum powder and pigment;

[0033] The HFC functional coating 14 further includes a transparent paint and an auxiliary agent added to the transparent paint, the resin contained in the transparent paint is at least one of acrylic resin, alkyd resin, phenolic resin, and polyester resin, and the auxiliary agent is a fluorine-plus-silicon system.

[0034] See also Figure 2 , Figure 3 , and refer to Figure 1 , Figure 2 Shown is a flow chart of the method for preparing a hydrophobic coating for aluminum alloy wheels according to the present invention. Figure 3 The figure shows the water drop angle detection spectrum of the hydrophobic coating surface for aluminum alloy wheels of the present invention. The preparation method of the hydrophobic coating for aluminum alloy wheels comprises:

[0035] Executing step S1: pre-treating the surface of the aluminum alloy wheel without chromium;

[0036] Execute step S2: deposit a primer coating 11, a primer coating 12, and a color paint coating 13 on the surface of the aluminum alloy wheel in sequence by electrostatic spraying, and perform a curing process;

[0037] Execute step S3: deposit the HFC functional coating 14 on the outer surface of the color paint coating 13 by electrostatic spraying.

[0038] Depend on Figure 3 It can be seen that the water drop angle on the surface of the hydrophobic coating prepared by the method for preparing the hydrophobic coating for aluminum alloy wheels of the present invention is greater than 95°. More specifically, the water drop angle on the surface of the hydrophobic coating prepared by the method for preparing the hydrophobic coating for aluminum alloy wheels of the present invention is 97.8°.

[0039] As an implementation mode, more specifically, in step S2, a primer coating 11 is deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the thickness of the primer coating 11 is 80-120 μm. The process parameters are: powder discharge amount 60-70 g / min, voltage 45-70 KV, static electricity 45-60 μA, total gas volume 4.5-5 MPa, baking temperature 160-200 ° C, and baking time 10-30 min. Preferably, in the process parameters, the powder discharge is 65 g / min, the voltage is 50 KV, the static electricity is 50 μA, the total gas volume is 4.75 MPa, the baking temperature is 177 ° C, and the baking time is 15 min.

[0040] The primer coating 12 and the color paint coating 13 are deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the total thickness of the primer coating 12 and the color paint coating 13 is 15-50 μm. The process parameters are: baking temperature 140-160° C., and baking time 10-30 minutes. Preferably, the baking temperature is 145° C. and the baking time is 20 minutes.

[0041] In step S4, an HFC functional coating 14 is deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the thickness of the HFC functional coating 14 is 15 to 30 μm. The process parameters are: baking temperature 140 to 160°C, and baking time 10 to 30 minutes. Preferably, the baking temperature is 145°C and the baking time is 20 minutes. More specifically, the HFC functional coating 14 is prepared by using a transparent paint and adding an auxiliary agent to the transparent paint and stirring, the auxiliary agent ratio is 0.3% to 1%, the stirring speed is 1000r / min, and the stirring time is 5 to 15 minutes. Preferably, the auxiliary agent ratio is 0.5%, and the stirring time is 10 minutes. The transparent paint is at least one of acrylic resin and polyester resin, and the auxiliary agent is a fluorine-silicon system.

[0042] As a person skilled in the art, it is easy to understand that the HFC functional coating 14 on the surface of the hydrophobic coating of the aluminum alloy wheel of the present invention is combined with a transparent paint to prepare an HFC functional paint by virtue of the small intermolecular force of the auxiliary component and the low surface energy, and then deposited on the surface of the aluminum alloy wheel by electrostatic spraying to obtain the HFC functional coating 14. The components of the transparent paint include but are not limited to oil, resin, auxiliary agent, and additive. Among them, the resin is mainly at least one of acrylic resin, alkyd resin, phenolic resin, and polyester resin. The resins all have functional groups, such as C=C, C=0, C-OH, CH, etc. The auxiliary agent and the resin form ionic bonds or covalent bonds with the elements in the auxiliary agent and the functional groups through van der Waals force, molecular force, or even atomic force under certain conditions, and the HFC functional paint is obtained by relying on the characteristics of small intermolecular force and low surface energy of the auxiliary agent. After the HFC functional paint is cured, the surface has a hydrophobic effect, and the water drop angle is greater than 95°.

[0043] Obviously, the hydrophobic coating for aluminum alloy wheels of the present invention can not only meet all paint film tests of existing aluminum alloy wheels, but also achieve obvious hydrophobic effect, improve the anti-fouling ability of the wheel hub surface, make it easy to clean, and increase the added value of wheel hub coating.

[0044] In summary, the hydrophobic coating for aluminum alloy wheels of the present invention can not only meet all paint film tests of existing aluminum alloy wheels, but also achieve obvious hydrophobic effect, improve the anti-fouling ability of the wheel hub surface, be easy to clean, and increase the added value of wheel hub coating.

[0045] Those skilled in the art will appreciate that various modifications and variations may be made to the present invention without departing from the spirit or scope of the present invention. Therefore, if any modification or variation falls within the scope of protection of the appended claims and equivalents, it is considered that the present invention covers these modifications and variations.

Claims

1. A hydrophobic coating for an aluminum alloy wheel, characterized in that: The hydrophobic coating for aluminum alloy wheels comprises: a base powder coating, a primer coating, a color paint coating, and an HFC functional coating which are sequentially stacked from the inside to the outside with the aluminum alloy wheel as the base, wherein: The base powder coating further comprises a base powder resin, a curing agent, a pigment filler and an auxiliary agent, wherein the base powder resin is a dual system of epoxy resin and polyester resin, wherein the epoxy resin and the polyester resin are curing agents for each other, the pigment filler is barium sulfate and carbon black, and the auxiliary agent is a leveling agent, a breathable agent, a brightener and a hardener; The primer coating further comprises a primer resin, a dispersant, a pigment filler, a cosolvent, water, a wetting and leveling agent, a defoamer, an additive and a thickener, and the primer resin is an epoxy resin system; The paint coating further comprises paint resin, solvent, filler, and additives, wherein the filler is aluminum powder and pigment; The HFC functional coating further comprises a transparent paint and an auxiliary agent added to the transparent paint, the resin contained in the transparent paint is at least one of acrylic resin, alkyd resin, phenolic resin and polyester resin, and the auxiliary agent is a fluorine-plus-silicon system.

2. The hydrophobic coating for aluminum alloy wheels according to claim 1, characterized in that: The water drop angle on the surface of the hydrophobic coating for aluminum alloy wheels is greater than 95°.

3. The hydrophobic coating for aluminum alloy wheels according to claim 2, characterized in that: The water drop angle on the surface of the hydrophobic coating for aluminum alloy wheels is 97.8°.

4. The hydrophobic coating for aluminum alloy wheels according to claim 1, characterized in that: The thickness of the primer coating is 80-120 μm.

5. The hydrophobic coating for aluminum alloy wheels according to claim 1, characterized in that: The total thickness of the primer coating and the color paint coating is 30 to 60 μm.

6. The hydrophobic coating for aluminum alloy wheels according to claim 1, characterized in that: The thickness of the HFC functional coating is 15 to 30 μm.

7. A method for preparing a hydrophobic coating for an aluminum alloy wheel as claimed in claim 1, characterized in that: The method for preparing the hydrophobic coating for aluminum alloy wheels comprises: Executing step S1: pre-treating the surface of the aluminum alloy wheel without chromium; Executing step S2: depositing a primer coating, a primer coating, and a color paint coating on the surface of the aluminum alloy wheel in sequence by electrostatic spraying, and performing a curing process; Execute step S3: deposit the HFC functional coating on the outer surface of the color paint coating by electrostatic spraying.

8. The method for preparing a hydrophobic coating for an aluminum alloy wheel as claimed in claim 7, characterized in that: In step S2, a base powder coating is deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the process parameters are: powder spraying amount 60-70 g / min, voltage 45-70 KV, static electricity 45-60 μA, total gas volume 4.5-5 MPa, baking temperature 160-200°C, and baking time 10-30 min.

9. The method for preparing a hydrophobic coating for an aluminum alloy wheel according to claim 7, characterized in that: The primer coating and the color paint coating are deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the process parameters are: baking temperature 140-160°C, and baking time 10-30 minutes.

10. The method for preparing a hydrophobic coating for an aluminum alloy wheel according to claim 7, characterized in that: The HFC functional coating is deposited on the surface of the aluminum alloy wheel by electrostatic spraying, and the process parameters are: baking temperature 140-160°C, and baking time 10-30 minutes.

11. The method for preparing a hydrophobic coating for an aluminum alloy wheel according to claim 10, characterized in that: The HFC functional coating is prepared by using a transparent paint and adding an auxiliary agent to the transparent paint and stirring, wherein the proportion of the auxiliary agent is 0.3% to 1%, the stirring speed is 1000 r / min, and the stirring time is 10 to 15 minutes.

Citation Information

Patent Citations

  • Preparation of branched hydrophobic auxiliary agent

    CN105482073A

  • Aluminum alloy surface coating and method for forming coating

    CN106423805A

  • Process for realizing corrosion prevention and mirror surface during coating of aluminum alloy wheels

    CN110328129A

  • Aluminum wheel coating and application thereof