High-adhesion resin condensate for quartz glass surface and preparation method of high-adhesion resin condensate
By using high adhesion resin cured substances composed of component A and component B at a mass ratio of 1:1.5 to 1:0.4 on the surface of quartz glass, the adhesion and wear resistance are improved by hydrogen bonds and chemical bonds, and traditional coatings are solved. The low adhesion of the layer and the water mist layer problems have achieved resin cured substances with high adhesion and wear resistance.
Patent Information
- Application Number
- CN202411031735.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
Due to its high finish and hydrophilicity, traditional organic coatings are difficult to adhere, resulting in low adhesion and easy to form a water mist layer, affecting the stability of the coating.
The high adhesion resin cured product consisting of a mass ratio of 1:1.5 to 1:0.4 with component A and component B, including vegetable oleic acid epoxy resin, hydroxy polyester resin, isocyanate polymer and isocyanate silane coupler Coupling agents form high adhesion and wear resistance through hydrogen bonding and chemical bonding.
The surface of quartz glass has high adhesion and wear resistance, with adhesion reaching more than 15MPa, and the mass loss after the wear resistance test is ≤5mg, solving the problems of low adhesion and water mist layer of traditional coatings.
Smart Images

Figure CN118931321A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass coatings, and in particular to a high-adhesion resin cured product for a quartz glass surface and a preparation method thereof. Background Art
[0002] Quartz glass materials are widely used in various industries due to their high temperature resistance, good thermal shock resistance and high chemical stability, especially in industrial fields such as electric light sources, lasers, optical instruments, and electrical equipment.
[0003] With the development of science and technology, clustered and functionalized materials are forming a large-scale technology industry group. Quartz glass has been proposed to have more functional requirements, but the structural characteristics and chemical composition of quartz glass itself limit its functional application prospects. In order to enhance the multifunctional characteristics of glass and make it suitable for more application scenarios, coating the surface of quartz glass with coating materials is one of the most effective ways to give glass functional requirements. Glass surface coating refers to the formation of a thin film layer on the surface of quartz glass through physical vapor deposition, chemical vapor deposition, sputtering or spraying and other processing techniques. This thin film layer can improve the physical or chemical properties of quartz glass, thereby meeting the functional or specific use requirements.
[0004] But first of all, because quartz glass is a special structure containing only a single component of silicon dioxide, its surface finish is relatively high. Traditional organic coatings are difficult to adhere to its surface by physical action alone. Usually, the adhesion of traditional organic coatings on the surface of quartz glass is only below 3MPa. Secondly, quartz glass is also an inorganic material with hydrophilic properties. Under normal circumstances, the surface of quartz glass is easily combined with water in the air to form a layer of water mist on its surface, which is also one of the important reasons for the low adhesion of organic coating materials on its surface. Summary of the invention
[0005] The invention provides a high-adhesion coating for a quartz glass surface and a preparation method thereof. The high-adhesion coating for a quartz glass surface has high adhesion and good wear resistance on the quartz glass surface, solving the problem that traditional organic coatings are difficult to adhere to the glass surface.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a high-adhesion resin cured product for a quartz glass surface, characterized in that it is composed of component A and component B in a mass ratio of 1:1.5 to 1:0.4;
[0008] Among them, component A includes, by mass:
[0009] 60-77 parts of vegetable oleic acid ring-opening epoxy resin;
[0010] 23-40 parts of hydroxy polyester resin;
[0011] 30-50 parts of xylene;
[0012] Among them, component B includes, by mass:
[0013] 60-80 parts of isocyanate polymer;
[0014] 5-15 parts of isocyanate silane coupling agent;
[0015] 5 to 35 parts of n-butyl acetate.
[0016] Preferably, the vegetable oil acid ring-opening epoxy resin comprises, in parts by mass:
[0017]
[0018] Preferably, the preparation method of the vegetable oil acid ring-opening epoxy resin comprises the following steps: mixing vegetable oil acid, bisphenol F epoxy resin, bisphenol A epoxy resin, Novolek epoxy resin, dibasic acid modified epoxy resin, aminosilane coupling agent and solvent, heating to 130°C to 150°C under inert gas protection, and keeping the temperature for reaction for 6 to 12 hours to obtain the vegetable oil acid ring-opening epoxy resin.
[0019] Preferably, the acid value of the vegetable oil acid is 190-205, the epoxy equivalent of bisphenol F epoxy resin is 160-200, the epoxy equivalent of bisphenol A epoxy resin is 500-1000, the epoxy equivalent of Novolek epoxy resin is 170-220, and the epoxy equivalent of dibasic acid modified epoxy resin is 230-700.
[0020] Preferably, the aminosilane coupling agent is one or two of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltrimethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxysilane, bis(3-trimethoxysilylpropyl)amine, and bis(3-triethoxysilylpropyl)amine.
[0021] Preferably, the solvent is one or more of n-amyl acetate, methyl isobutyl ketone and cyclohexanone.
[0022] Preferably, the isocyanate silane coupling agent is one of 3-isocyanate propyl trimethoxy silane and 3-isocyanate propyl triethoxy silane.
[0023] Preferably, the hydroxyl content in the hydroxy polyester resin is 6.6% to 8.2%, and the -NCO content in the isocyanate polymer is 15% to 32%.
[0024] Preferably, the structural formula of the vegetable oil acid ring-opening epoxy resin is:
[0025]
[0026] The method for preparing the high-adhesion resin cured product for the quartz glass surface comprises the following steps:
[0027] (1) Mixing vegetable oil acid ring-opening epoxy resin, hydroxy polyester resin and xylene, stirring for 5 to 10 minutes and then filtering to obtain component A;
[0028] (2) mixing the isocyanate polymer, the isocyanate silane coupling agent and n-butyl acetate, stirring for 5 to 10 minutes and filtering to obtain component B;
[0029] (3) Component A and component B are mixed in proportion and stirred evenly to obtain a high-adhesion resin cured product for the quartz glass surface.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) The high-adhesion resin cured product for quartz glass surface obtained by the present invention has excellent adhesion on the quartz glass surface and good wear resistance. The adhesion between the cured product and the quartz glass surface can reach 15 MPa or more, which is a manifestation of high adhesion (usually, 10 MPa or more is considered high adhesion). After the resin cured product of the present invention is subjected to a 500 g*1000 r wear test, the mass loss after wear is ≤5 mg.
[0032] (2) The present invention adopts vegetable oleic acid ring-opening epoxy resin, and ensures the degree of ring-opening reaction by strictly controlling the feeding ratio between vegetable oleic acid and epoxy resin. The vegetable oleic acid ring-opening epoxy resin contains a large number of polar functional groups in its molecular structure, which can form hydrogen bonds with the surface of quartz glass, thereby improving the bonding strength between the cured product and the substrate, so that the resin cured product obtained by the present invention has excellent adhesion on the surface of quartz glass; the bisphenol F type epoxy resin and the dibasic acid modified epoxy resin after ring opening can provide good flexibility for the entire cured product, ensuring that the internal stress formed by the A and B components during the curing process can be effectively released; the bisphenol A type epoxy resin and the Novolek epoxy resin after ring opening have more hydroxyl groups, and after the cross-linking reaction of the A and B components, the cohesive strength of the resin cured product obtained by the present invention is greatly improved, so that the resin cured product obtained by the present invention has excellent wear resistance.
[0033] (3) The present invention adds an aminosilane coupling agent to the synthesis reaction of the vegetable oil acid ring-opening epoxy resin. After the amino group undergoes a ring-opening reaction with the epoxy resin, a silane structure can be introduced into the main resin molecular structure. After the epoxy resin is ring-opened by the vegetable oil acid, a hydroxyl structure is generated. Since the second component contains an isocyanate silane coupling agent, the isocyanate group reacts with the hydroxyl group. The silane structure is introduced into the resin cured product. The silane structure can react with moisture in the air to form a silanol group. The silanol group can undergo a cross-linking reaction with the active hydroxyl group on the surface of the quartz glass, and then the resin cured product and the quartz glass surface are connected in a chemical bond manner, forming the quartz glass and the resin cured product into an organic whole, thereby greatly improving the adhesion of the resin cured product and the quartz glass, and at the same time effectively solving the problem of the loss of adhesion caused by the formation of a water mist layer on the surface of the quartz glass.
[0034] (4) After the epoxy resin ring-opened by vegetable oil acid in the present invention is mixed with a hydroxyl polyester resin having a hydroxyl content of 6.6% to 8.2%, and then cured with an isocyanate polymer, the formed cured product has the characteristics of high cross-linking density and high hardness. At the same time, the molecular structure of the cured product contains flexible structural segments. The molecular structure of this resin cured product has the characteristics of both hardness and toughness, so that the cured product has excellent wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0037] Figure 1 This is the infrared spectrum of epoxy resin.
[0038] Figure 2 This is the infrared spectrum of vegetable oil acid ring-opening epoxy resin after 4 hours of reaction.
[0039] Figure 3 This is the infrared spectrum of vegetable oil acid ring-opening epoxy resin after 8 hours of reaction.
[0040] Figure 4 This is a photograph of a coating material prepared by using a high-adhesion resin cured product on the surface of quartz glass in the present invention before a wear resistance test.
[0041] Figure 5 The following is a photograph of a coating material prepared by using a high-adhesion resin cured product on the surface of quartz glass according to the present invention after a wear resistance test. DETAILED DESCRIPTION
[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Example 1
[0044] A high-adhesion resin cured product for a quartz glass surface, comprising component A and component B in a mass ratio of 2:1;
[0045] Component A comprises, by weight: 70 parts of vegetable oil acid ring-opening epoxy resin, 30 parts of hydroxy polyester resin having a hydroxyl content of 7.5%, and 35 parts of xylene;
[0046] Component B comprises, by mass: 66 parts of an isocyanate polymer having an NCO content of 20.5%, 8 parts of 3-isocyanatepropyltriethoxysilane, and 20 parts of n-butyl acetate.
[0047] The method for preparing a high-adhesion resin cured product for a quartz glass surface comprises the following steps:
[0048] (1) 70 parts of the synthesized vegetable oil acid ring-opening epoxy resin, 30 parts of a hydroxy polyester resin having a hydroxyl content of 7.5%, and 35 parts of xylene are added to a pull cylinder, stirred for 10 minutes, and then filtered to obtain component A;
[0049] (2) adding 66 parts of an isocyanate polymer having an -NCO content of 20.5%, 8 parts of 3-isocyanatepropyltriethoxysilane, and 20 parts of n-butyl acetate into a pull cylinder, stirring for 5 minutes, and filtering the material to obtain component B;
[0050] (3) Component A and component B are mixed in a mass ratio of 2:1 and stirred evenly to obtain a high-adhesion resin cured product for the quartz glass surface.
[0051] In this embodiment, the preparation method of the vegetable oil acid ring-opening epoxy resin is as follows: 40 parts of vegetable oil acid with an acid value of 200, 20 parts of bisphenol F epoxy resin with an epoxy equivalent of 180, 41 parts of bisphenol A epoxy resin with an epoxy equivalent of 675, 8 parts of Novolek epoxy resin with an epoxy equivalent of 190, 22 parts of dibasic acid modified epoxy resin with an epoxy equivalent of 460, 10 parts of N-2-aminoethyl-3-aminopropyltriethoxysilane, 100 parts of n-pentyl acetate, and 30 parts of cyclohexanone are mixed, and the mixture is heated to 130° C. under the protection of an inert gas, and the mixture is kept warm for reaction for 12 hours to obtain a vegetable oil acid ring-opening epoxy resin having the structural formula:
[0052]
[0053] Example 2
[0054] A high-adhesion resin cured product for a quartz glass surface, comprising component A and component B in a mass ratio of 1:1.5;
[0055] Component A comprises, by weight: 65 parts of vegetable oil acid ring-opening epoxy resin, 40 parts of hydroxy polyester resin having a hydroxyl content of 8.2%, and 40 parts of xylene;
[0056] Component B comprises, by mass: 63 parts of an isocyanate polymer having an NCO content of 32%, 12 parts of 3-isocyanatepropyltrimethoxysilane, and 8 parts of n-butyl acetate.
[0057] The method for preparing a high-adhesion resin cured product for a quartz glass surface comprises the following steps:
[0058] (1) 65 parts of the synthesized vegetable oil acid ring-opening epoxy resin, 40 parts of a hydroxy polyester resin having a hydroxyl content of 8.2%, and 40 parts of xylene are added to a pull cylinder, stirred for 5 minutes, and then filtered to obtain component A.
[0059] (2) Add 63 parts of an isocyanate polymer having an -NCO content of 32%, 12 parts of 3-isocyanatepropyltrimethoxysilane, and 8 parts of n-butyl acetate into a pull cylinder, stir for 10 minutes, and then filter the material to obtain component B.
[0060] (3) Component A and component B are mixed in a mass ratio of 1:1.5, and stirred evenly to obtain a high-adhesion resin cured product for the quartz glass surface.
[0061] In this embodiment, the preparation method of the vegetable oil acid ring-opening epoxy resin is as follows: 55 parts of vegetable oil acid with an acid value of 200, 18 parts of bisphenol F epoxy resin with an epoxy equivalent of 200, 50 parts of bisphenol A epoxy resin with an epoxy equivalent of 900, 10 parts of Novolek epoxy resin with an epoxy equivalent of 170, 23 parts of dibasic acid modified epoxy resin with an epoxy equivalent of 230, 6 parts of N-2-aminoethyl-3-aminopropyltrimethoxysilane, 70 parts of n-pentyl acetate, and 80 parts of cyclohexanone are mixed, the temperature is raised to 150° C. under the protection of inert gas, and the reaction is kept warm for 6 hours to obtain the vegetable oil acid ring-opening epoxy resin.
[0062] Example 3
[0063] A high-adhesion resin cured product for a quartz glass surface, comprising component A and component B in a mass ratio of 1:1;
[0064] Component A comprises, by weight: 74 parts of vegetable oil acid ring-opening epoxy resin, 32 parts of hydroxy polyester resin having a hydroxyl content of 6.9%, and 50 parts of xylene;
[0065] Component B comprises, by mass: 61 parts of an isocyanate polymer having an NCO content of 19.5%, 7 parts of 3-isocyanatepropyltriethoxysilane, and 15 parts of n-butyl acetate.
[0066] The method for preparing a high-adhesion resin cured product for a quartz glass surface comprises the following steps:
[0067] (1) adding 74 parts of synthesized vegetable oil acid ring-opening epoxy resin, 32 parts of hydroxy polyester resin with a hydroxyl content of 6.9%, and 50 parts of xylene into a pull cylinder, stirring for 8 minutes, and then filtering the material to obtain a high-adhesion wear-resistant resin component A for quartz glass surface;
[0068] (2) adding 61 parts of an isocyanate polymer having an -NCO content of 19.5%, 7 parts of 3-isocyanatepropyltriethoxysilane, and 15 parts of n-butyl acetate into a pull cylinder, stirring for 8 minutes, and filtering the material to obtain a high-adhesion wear-resistant resin component B for a quartz glass surface;
[0069] (3) Component A and component B are mixed in a mass ratio of 1:1 and stirred evenly to obtain a high-adhesion resin cured product for the quartz glass surface.
[0070] In this embodiment, the preparation method of the vegetable oil acid ring-opening epoxy resin is as follows: 60 parts of vegetable oil acid with an acid value of 200, 25 parts of bisphenol F epoxy resin with an epoxy equivalent of 170, 43 parts of bisphenol A epoxy resin with an epoxy equivalent of 625, 8 parts of Novolek epoxy resin with an epoxy equivalent of 200, 23 parts of dibasic acid modified epoxy resin with an epoxy equivalent of 440, 7 parts of bis(3-triethoxysilylpropyl)amine, 53 parts of methyl isobutyl ketone, and 58 parts of cyclohexanone are mixed, the temperature is raised to 140°C under the protection of an inert gas, and the reaction is kept warm for 9 hours to obtain the vegetable oil acid ring-opening epoxy resin.
[0071] refer to Figure 4 and Figure 5 The quartz glass surfaces of Examples 1 to 3 were painted with high-adhesion resin curing materials to prepare curing films, and performance tests were performed after drying for 7 days. The test results are shown in Table 1.
[0072] Table 1 Performance test table
[0073]
[0074]
[0075] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0076] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A high-adhesion resin cured product for quartz glass surface, characterized in that: It is composed of component A and component B in a mass ratio of 1:1.5 to 1:0.4; Among them, component A includes, by mass: 60-77 parts of vegetable oleic acid ring-opening epoxy resin; 23-40 parts of hydroxy polyester resin; 30-50 parts of xylene; Among them, component B includes, by mass: 60-80 parts of isocyanate polymer; 5-15 parts of isocyanate silane coupling agent; 5 to 35 parts of n-butyl acetate.
2. The high-adhesion resin cured product for quartz glass surface according to claim 1, characterized in that: The vegetable oil acid ring-opening epoxy resin comprises, in parts by mass:
3. The high-adhesion resin cured product for quartz glass surface according to claim 2, characterized in that: The preparation method of the vegetable oil acid ring-opening epoxy resin comprises the following steps: mixing vegetable oil acid, bisphenol F epoxy resin, bisphenol A epoxy resin, Novolek epoxy resin, dibasic acid modified epoxy resin, aminosilane coupling agent and solvent, heating to 130° C. to 150° C. under the protection of inert gas, and keeping the temperature for reaction for 6 to 12 hours to obtain the vegetable oil acid ring-opening epoxy resin.
4. The high-adhesion resin cured product for quartz glass surface according to claim 2, characterized in that: The acid value of the vegetable oil acid is 190-205, the epoxy equivalent of the bisphenol F epoxy resin is 160-200, the epoxy equivalent of the bisphenol A epoxy resin is 500-1000, the epoxy equivalent of the Novolek epoxy resin is 170-220, and the epoxy equivalent of the dibasic acid modified epoxy resin is 230-700.
5. The high-adhesion resin cured product for quartz glass surface according to claim 2, characterized in that: The aminosilane coupling agent is one or two of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-aminoethyl-3-aminopropyltrimethoxysilane, N-2-aminoethyl-3-aminopropyltriethoxysilane, bis(3-trimethoxysilylpropyl)amine, and bis(3-triethoxysilylpropyl)amine.
6. The high-adhesion resin cured product for quartz glass surface according to claim 2, characterized in that: The solvent is one or more of n-amyl acetate, methyl isobutyl ketone and cyclohexanone.
7. The high-adhesion resin cured product for quartz glass surface according to claim 1, characterized in that: The isocyanate silane coupling agent is one of 3-isocyanate propyl trimethoxy silane and 3-isocyanate propyl triethoxy silane.
8. The high-adhesion resin cured product for quartz glass surface according to claim 1, characterized in that: The hydroxyl content in the hydroxy polyester resin is 6.6% to 8.2%, and the -NCO content in the isocyanate polymer is 15% to 32%.
9. The high-adhesion resin cured product for quartz glass surface according to claim 1, characterized in that: The structural formula of the vegetable oil acid ring-opening epoxy resin is:
10. The method for preparing a high-adhesion resin cured product for quartz glass surface according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Mixing vegetable oil acid ring-opening epoxy resin, hydroxy polyester resin and xylene, stirring for 5 to 10 minutes and then filtering to obtain component A; (2) mixing the isocyanate polymer, the isocyanate silane coupling agent and n-butyl acetate, stirring for 5 to 10 minutes and filtering to obtain component B; (3) Component A and component B are mixed in proportion and stirred evenly to obtain a high-adhesion resin cured product for the quartz glass surface.
Citation Information
Patent Citations
Nanometer modified high-solid polyurethane anti-corrosive paint and preparation method thereof
CN101565589A
Preparation method of heavy corrosion protection primer resin
CN106634453A
Glass printing ink
CN106833111A