Nano titanium modified flake zinc powder anticorrosive paint
Through nano-titanium modified scale zinc powder anticorrosion coating, combined with components such as water-based polyester resin and epoxy resin, the problem of poor corrosion resistance in harsh environments is solved, and higher corrosion resistance and mechanical properties are achieved. It has the characteristics of corrosion resistance of acid, alkali, salt and other media, oil, water, and aging.
Patent Information
- Application Number
- CN202410916683.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing environmentally friendly anticorrosion coatings are difficult to meet the long-term anticorrosion needs of the equipment surface under harsh corrosion environments. The coatings are prone to falling off and have poor corrosion resistance and high temperature resistance.
Using nano-titanium modified scale zinc powder anticorrosion coating, aqueous polyester resin, epoxy resin, scale zinc powder, nano-titanium, nano-titanium dioxide and other components, the scale zinc powder is formed through specific ingredients and processes to improve the coating. Conductivity and corrosion resistance.
It significantly improves the corrosion resistance and mechanical properties of the paint, enhances the electrochemical corrosion effect of the paint film, and has the characteristics of corrosion resistance of acid, alkali, salt and other media, oil, water, and aging resistance, strong adhesion, good impact resistance, and cost Low and stable performance.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmentally friendly anti-corrosion coatings, and specifically relates to a nano-titanium modified flaky zinc powder anti-corrosion coating. Background Art
[0002] In the prior art, many environmental protection equipment are exposed to wind and rain for a long time, and the anti-corrosion performance of the equipment surface is required to be extremely high; there are many means to prevent the corrosion of metal materials, such as the use of corrosion-resistant metal materials, cathodic protection, corrosion inhibitors and metal protective coatings. Practice has proved that among the above metal anti-corrosion methods, the use of environmentally friendly anti-corrosion coatings to protect easily corroded metal materials is the most economical, effective and widely used anti-corrosion method. Conventional anti-corrosion coatings play an anti-corrosion role on metals under general conditions, thereby increasing the service life of non-ferrous metals; however, conventional anti-corrosion coatings cannot be used in relatively harsh corrosive environments, and it is difficult to meet the user's demand for the anti-corrosion ability of coatings. After a period of use, the surface of environmental protection equipment under the anti-corrosion coating will fall off and the anti-corrosion performance is poor.
[0003] Anti-corrosion coatings are mainly applied on the surface of objects to form a thin film or to play a protective or decorative role. For example, the existing patent document CN108219607 A discloses an anti-corrosion water-based coating. The obtained water-based coating has good corrosion resistance and can be applied to coatings in various industries. However, the prior art still has the problem that after the coating is applied to the surface of an object, as the environment changes, the corrosion resistance and high temperature resistance are poor. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a nano-titanium modified flake zinc powder anti-corrosion coating in view of the shortcomings of the background technology.
[0005] The present invention adopts the following technical solutions to solve the above technical problems:
[0006] A nano-titanium modified flaky zinc powder anticorrosive coating comprises the following ingredients in parts by weight: 20-35 parts of waterborne polyester resin, 10-15 parts of epoxy resin, 20-50 parts of flaky zinc powder, 10-15 parts of nano-titanium, 5-10 parts of nano-titanium dioxide, 12-18 parts of carbon black, 3-6 parts of zinc phosphate, 3-6 parts of calcium carbonate, 3-6 parts of silicon dioxide, 5-10 parts of sodium fluorosilicate, 30-50 parts of acrylic emulsion, 8-20 parts of curing agent and 10-50 parts of solvent.
[0007] As a further preferred embodiment of a nano-titanium modified flake zinc powder anti-corrosion coating of the present invention, the flake zinc powder uses atomized spherical zinc powder with a particle size less than 325 mesh as a raw material, steel balls are added at a weight ratio of 10-20:1 between steel balls and zinc powder, and 1-3% of the weight of the zinc powder is added as a grinding aid and a surface modifier to obtain material a; the steel balls are steel balls with diameters of φ20 mm and φ12 mm, and the number ratio of the two types of steel balls is 1:3.
[0008] As a further preferred embodiment of the nano-titanium modified zinc flake anticorrosion coating of the present invention, the water-based polyester resin is a mixture of one or more of neopentyl glycol, adipic acid, phthalic acid, isophthalic anhydride, trimellitic anhydride, a catalyst, an antioxidant, a neutralizer and water.
[0009] As a further preferred embodiment of the nano-titanium modified zinc flake anti-corrosion coating of the present invention, the epoxy resin is one or a mixture of two or more of bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, hydroxymethyl bisphenol A type epoxy resin, bromine-modified diphenol propane epoxy resin, and graphene-modified epoxy resin.
[0010] As a further preferred embodiment of the nano-titanium modified zinc flake anti-corrosion coating of the present invention, the acrylic emulsion is composed of pure acrylic emulsion and silicone acrylic emulsion in a weight ratio of 1:2.
[0011] As a further preferred embodiment of the nano-titanium modified zinc flake anti-corrosion coating of the present invention, the curing agent is one or a mixture of two or more of aliphatic amines, aromatic amines, alicyclic amines or amine-modified curing agents.
[0012] As a further preferred embodiment of the nano-titanium modified zinc flake anticorrosion coating of the present invention, the solvent is a mixture of one of toluene, xylene, and styrene and one of n-butanol, isobutanol, tert-butanol, butanone, and cyclohexanone or more than two thereof.
[0013] Compared with the prior art, the present invention adopts the above technical solution and has the following technical effects:
[0014] The present invention discloses a nano-titanium modified flaky zinc powder anticorrosion coating. The components and contents of the nano-titanium modified flaky zinc powder anticorrosion coating are appropriate, so that the anticorrosion effect of the product is much better than that of the traditional spherical zinc powder. An appropriate amount of nano-titanium powder is added to the nano-titanium modified flaky zinc powder anticorrosion coating, thereby greatly improving the anticorrosion and mechanical properties of the coating, and at the same time increasing the conductivity of the flaky zinc powder coating, further improving the electrochemical anticorrosion effect of the paint film. The coating of the product of the present invention settles after being placed for a long time during construction, the coating is uniform, and the paint surface is smooth, so that it can be used as a primer or a topcoat. The nano-titanium modified flaky zinc powder anticorrosion coating of the present invention has low cost and stable performance. It not only has the unique function of being resistant to corrosion by media such as acid, alkali, and salt, but also has the characteristics of oil resistance, water resistance, and anti-aging, strong adhesion, good impact resistance, and good flexibility. DETAILED DESCRIPTION
[0015] The technical solution of the present invention is further described in detail below:
[0016] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.
[0017] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0018] A nano-titanium modified flaky zinc powder anticorrosive coating comprises the following ingredients in parts by weight: 20-35 parts of waterborne polyester resin, 10-15 parts of epoxy resin, 20-50 parts of flaky zinc powder, 10-15 parts of nano-titanium, 5-10 parts of nano-titanium dioxide, 12-18 parts of carbon black, 3-6 parts of zinc phosphate, 3-6 parts of calcium carbonate, 3-6 parts of silicon dioxide, 5-10 parts of sodium fluorosilicate, 30-50 parts of acrylic emulsion, 8-20 parts of curing agent and 10-50 parts of solvent.
[0019] The flake zinc powder uses atomized spherical zinc powder with a particle size of less than 325 mesh as raw material, and steel balls are added at a weight ratio of 1020:1 to zinc powder, and 13% of the weight of zinc powder is added to obtain material a; the steel balls are steel balls with diameters of φ20mm and φ12mm, and the number ratio of the two types of steel balls is 1:3.
[0020] The method for preparing flaky zinc powder of the present invention comprises the steps of batching, ball milling, drying and screening, and specifically comprises:
[0021] A. Ingredients: using atomized spherical zinc powder with a particle size of less than 325 mesh as raw material, adding steel balls with a weight ratio of 10-20:1 of zinc powder, and adding grinding aids and surface modifiers with a weight percentage of 1-3 of zinc powder to obtain material a;
[0022] B. Ball milling: Place material a in a ball mill, add 99% ethanol solution with a solid-liquid mass ratio of 1:5-6 times the volume concentration of material a, and perform ball milling to obtain material b;
[0023] C. Drying: Dry material b to constant weight;
[0024] D. Screening: The dried material b is classified by a cyclone classification system to obtain the target material.
[0025] The diameters of the steel balls are φ20 mm and φ12 mm respectively, and the quantity ratio thereof is 1:3.
[0026] The grinding aid is one or more of zinc stearate, stearic acid and aluminum stearate.
[0027] The surface modifier is one or more of sodium dodecylbenzene sulfonate, polyvinyl alcohol, titanate coupling agent or silane coupling agent.
[0028] The ball milling speed is 1000-2000r / min, and the ball milling time is 6-10h.
[0029] The drying is vacuum drying.
[0030] The drying temperature is 70-80°C.
[0031] Put 200g-325 mesh (i.e. less than 325 mesh) atomized spherical zinc powder, 3000g steel balls, 3g stearic acid, 3g polyvinyl alcohol, and 1000g ethanol with a volume concentration of 99% into a ball mill;
[0032] The speed of the ball mill was 1500 rpm, and the ball milling time was 6 h;
[0033] The ball-milled zinc powder is placed in a vacuum drying oven and dried at 70-80°C.
[0034] The dried zinc powder was classified by a cyclone classification system to obtain phosphorus flake zinc powder with an average particle size of D(50)=22.4 μm, a flake degree of 93%, and a diameter-to-thickness ratio of 47.
[0035] The waterborne polyester resin is one or a mixture of two or more of neopentyl glycol, adipic acid, phthalic acid, isophthalic anhydride, trimellitic anhydride, a catalyst, an antioxidant, a neutralizer and water.
[0036] The epoxy resin is one or a mixture of two or more of bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, hydroxymethyl bisphenol A type epoxy resin, bromine-modified diphenol propane epoxy resin, and graphene-modified epoxy resin.
[0037] The acrylic emulsion is composed of pure acrylic emulsion and silicone acrylic emulsion in a weight ratio of 1:2.
[0038] The curing agent is one or a mixture of two or more of aliphatic amine, aromatic amine, alicyclic amine or amine-modified curing agent.
[0039] The solvent is one of toluene, xylene and styrene and one of n-butanol, isobutanol, tert-butanol, butanone and cyclohexanone or a mixture of two or more thereof.
[0040] A method for preparing a nano-titanium modified zinc flake anti-corrosion coating, specifically comprising the following steps:
[0041] Step 1, ingredients: using atomized spherical zinc powder with a particle size of less than 325 mesh as a raw material, adding steel balls at a weight ratio of 1020:1 to zinc powder, and adding 1 3% of the weight of zinc powder as a grinding aid and a surface modifier to obtain material a; the steel balls are steel balls with diameters of φ20 mm and φ12 mm, and the ratio of the two types of steel balls is 1:3;
[0042] Ball milling: place material a in a ball mill, add a 99% ethanol solution with a solid-liquid mass ratio of 1:5:6 for ball milling, the speed of the ball mill is 1000-2000r / min, and the ball milling time is 6-10h to obtain material b;
[0043] Drying: Dry material b to constant weight;
[0044] Screening: The dried material b is classified by a cyclone classification system to obtain flake zinc powder;
[0045] Step 2, adding nano titanium, stirring and grinding in a grinder for 10-35 minutes, filtering and drying to obtain nano titanium modified flake zinc powder;
[0046] Step 3, slowly drop epoxy resin and acrylic emulsion into epoxy resin, raise the temperature to 60-80° C., react at constant temperature for 10-40 minutes, cool to 40-50° C., add nano-titanium dioxide, and perform ultrasonic treatment for 15-20 minutes to obtain a mixed emulsion;
[0047] Step 4, adding the mixed emulsion in step 3, the nano-titanium modified flake zinc powder in step 2 and 12 to 18 parts of carbon black, zinc phosphate, calcium carbonate, silicon dioxide, sodium fluorosilicate, a curing agent, and a solvent into a stirring container and dispersing at a high speed of 900 to 1400 rpm for 1 to 3 hours to obtain a corrosion-resistant coating;
[0048] Step 5, placing the barrel to be filled under the processing device, and quickly adding the corrosion-resistant coating into the barrel through the processing device;
[0049] Step 6, sealing the storage barrel to obtain the barreled corrosion-resistant coating.
[0050] The components and contents of the invented nano-titanium modified flaky zinc powder anti-corrosion coating are appropriate, so that the anti-corrosion effect of the product is much better than that of the traditional spherical zinc powder; an appropriate amount of nano-titanium powder is added to the nano-titanium modified flaky zinc powder anti-corrosion coating, which can greatly improve the corrosion resistance and mechanical properties of the coating, and at the same time increase the conductivity of the flaky zinc powder coating, further improving the electrochemical anti-corrosion effect of the paint film. The coating of the product of the present invention settles after being placed for a period of time during construction, the coating is uniform, and the paint surface is smooth, so it can be used as a primer or a topcoat. The nano-titanium modified flaky zinc powder anti-corrosion coating of the present invention has low cost and stable performance. It not only has the unique function of being resistant to corrosion by media such as acid, alkali, and salt, but also has the characteristics of oil resistance, water resistance, and anti-aging, strong adhesion, good impact resistance, and good flexibility.
[0051] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A nano-titanium modified zinc flake anti-corrosion coating, characterized in that: The invention comprises the following ingredients in parts by weight: 20-35 parts of water-based polyester resin, 10-15 parts of epoxy resin, 20-50 parts of flake zinc powder, 10-15 parts of nano titanium, 5-10 parts of nano titanium dioxide, 12-18 parts of carbon black, 3-6 parts of zinc phosphate, 3-6 parts of calcium carbonate, 3-6 parts of silicon dioxide, 5-10 parts of sodium fluorosilicate, 30-50 parts of acrylic emulsion, 8-20 parts of curing agent and 10-50 parts of solvent.
2. The nano-titanium modified zinc flake anticorrosion coating according to claim 1, characterized in that: The flake zinc powder uses atomized spherical zinc powder with a particle size of less than 325 mesh as raw material, and steel balls are added in a weight ratio of 10-20:1, and 1-3% of the weight of the zinc powder is added. Grinding aids and surface modifiers are obtained to obtain material a; the steel balls are steel balls with diameters of φ20mm and φ12mm, and the number ratio of the two types of steel balls is 1:
3.
3. The nano-titanium modified zinc flake anticorrosion coating according to claim 1, characterized in that: The waterborne polyester resin is one or a mixture of two or more of neopentyl glycol, adipic acid, phthalic acid, isophthalic anhydride, trimellitic anhydride, a catalyst, an antioxidant, a neutralizer and water.
4. The nano-titanium modified zinc flake anticorrosion coating according to claim 1, characterized in that: The epoxy resin is one or a mixture of two or more of bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, hydroxymethyl bisphenol A type epoxy resin, bromine-modified diphenol propane epoxy resin, and graphene-modified epoxy resin.
5. The nano-titanium modified zinc flake anticorrosion coating according to claim 1, characterized in that: The acrylic emulsion is composed of pure acrylic emulsion and silicone acrylic emulsion in a weight ratio of 1:
2.
6. The nano-titanium modified zinc flake anticorrosion coating according to claim 1, characterized in that: The curing agent is one or a mixture of two or more of aliphatic amine, aromatic amine, alicyclic amine or amine-modified curing agent.
7. The nano-titanium modified zinc flake anticorrosion coating according to claim 1, characterized in that: The solvent is one of toluene, xylene and styrene and one of n-butanol, isobutanol, tert-butanol, butanone and cyclohexanone or a mixture of two or more thereof.
Citation Information
Patent Citations
Anti-corrosion water-based paint