Stain-resistant anti-dazzle coating, adhesive tape, preparation method and application
By using hexafunctional fluorine-containing silicone special modified acrylate oligomers, polyfunctional acrylate monomers and nano-scale silica particles in anti-glare film tape, a scratch-resistant, wear-resistant and stain-resistant coating is solved The existing anti-glare film tape has poor scratch resistance and easy imprinting problems, achieving high stain resistance and anti-glare effects.
Patent Information
- Application Number
- CN202411027452.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing anti-glare film tape has poor scratch resistance and is prone to scratches. It is easy to leave fingerprints and oil marks when there are sweat stains or oil stains, which affects the aesthetics of the screen and may corrode the screen or screen protector.
The special modified acrylic oligomer with a multi-compartment acrylate monomer is used to form a cross-linked network structure through UV radiation, and the fluorosilic chain segments are migrated to the surface, combining nano-grade silica particles to improve coating The scratch, wear and stain resistance of the layer.
It achieves high stain resistance, wear resistance and glare resistance, enhances the surface strength and hardness of the coating, significantly improves the wetting properties of water and oil droplets, and ensures the cleanliness and durability of the screen.
Smart Images

Figure CN118931358A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesive tapes, and in particular to a stain-resistant anti-glare coating, an adhesive tape, and a preparation method and application thereof. Background Art
[0002] Nowadays, people are more and more inclined to travel by car, and numerous in-vehicle display devices have also brought comfort and convenience to drivers and passengers. Generally speaking, in order to prevent the impact of "glare" on drivers, anti-glare (Anti-Glare) treatment is performed on the surface of various in-vehicle display screens. The common practice is to stick anti-glare film tape on the outside, but the general anti-glare film tape has poor scratch resistance, and the screen of electronic products is easily scratched by sharp objects. In addition, when the user has sweat or oil stains on his hands, it is easy to leave fingerprints and oil stains after touching the screen, and these marks are difficult to wipe clean. If the treatment is slightly improper, it will dirty the entire screen and affect the appearance of the product. At the same time, these marks will slowly corrode the screen or screen protector over a long period of time.
[0003] In response to the above problems, the Chinese invention patent with patent number CN202010549817.X (publication number CN111826061B) discloses an anti-fouling and anti-glare coating and its preparation method. The anti-fouling and anti-glare coating comprises 5 to 30 parts of fluorosilicone modified acrylate polymer, 20 to 50 parts of a second acrylate polymer, 5 to 20 parts of a monofunctional active diluent, 5 to 20 parts of a multifunctional active diluent, 1 to 10 parts of anti-glare particles, and 1 to 5 parts of a photoinitiator. The invention relates to a coating composition comprising a fluorine-silicon modified acrylate polymer and 20 to 100 parts of a solvent; wherein the functionality of the fluorine-silicon modified acrylate polymer is 6 to 15, and the functionality of the second acrylate polymer is above 3. When the anti-fouling and anti-glare coating is cured to form a film layer, the fluorine and silicon elements in the fluorine-silicon modified acrylate polymer will be enriched on the surface of the film layer, so that the film layer has a low surface energy, thereby obtaining a hydrophobic and oleophobic surface property; and the added anti-glare particles can weaken the specular reflection of the film layer surface and enhance the diffuse reflection, thereby achieving the purpose of anti-glare.
[0004] The above patent obtains hydrophobic and oleophobic surface properties by enriching the fluorine and silicon elements in the fluorine-silicon modified acrylate polymer on the surface of the film layer, and the water drop angle is greater than 105°, but its anti-fouling effect needs to be further improved. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a stain-resistant and anti-glare coating with good stain-resistant, wear-resistant and anti-glare effects in view of the current status of the prior art.
[0006] The technical solution adopted by the present invention to solve the above-mentioned first technical problem is: a stain-resistant anti-glare coating, characterized in that it comprises the following components in percentage by weight:
[0007] Hexafunctional fluorine-containing silicon-modified acrylate oligomer 18.3-27.8%;
[0008] Hexafunctional acrylate monomer 5.5-12.3%;
[0009] Trifunctional acrylate monomer 2.2-12.3%;
[0010] Photoinitiator 1.5-2.5%;
[0011] Leveling agent 0.1~0.3%;
[0012] Anti-glare particles 2.0% to 2.5%;
[0013] Hardened particles 12.3-22.9%;
[0014] Organic solvent 42.9%~52.5%.
[0015] The fluorosilicone special modified acrylate oligomer is at least one of polyester acrylate or polyurethane acrylate with a functionality of ≥3;
[0016] The acrylate monomer is selected from at least one of dipentaerythritol hexaacrylate, 1,6-hexanediol diacrylate, ethylene glycol diacrylate, pentanediol diacrylate, trimethylolpropane triacrylate, trimethylolpentane trimethacrylate, 1,3-propylene glycol dimethacrylate, dipropylene glycol diacrylate, dipentaerythritol triacrylate and 2-ethylpentaerythritol triacrylate.
[0017] Preferably, the anti-fouling anti-glare coating comprises the following components in percentage by weight:
[0018] Hexafunctional fluorine-containing silicon-modified special acrylate oligomer 22.9%;
[0019] Hexafunctional acrylate monomer 8.8%;
[0020] Trifunctional acrylate monomer 3.5%;
[0021] Photoinitiator 1.8%;
[0022] Leveling agent 0.15%;
[0023] Anti-glare particles 2.0%;
[0024] Hardened particles 17.6%;
[0025] Organic solvent 43.3%.
[0026] Preferably, the organic solvent comprises methyl isobutyl ketone and propylene glycol methyl ether, wherein the mass ratio of methyl isobutyl ketone to propylene glycol methyl ether is (3:2).
[0027] Preferably, the leveling agent is EFKA3030, which includes polyether modified siloxane. The main component of the leveling agent is polyether modified siloxane, which can effectively promote leveling and improve slip, thereby improving the scratch resistance of the coating. In addition, compared with pure siloxane without modification, EFKA3030 has good solvent compatibility and has very good anti-cratering and low foam stabilizing effects.
[0028] Preferably, the photoinitiator is one or more combinations of 2-hydroxy-2-methyl-1-phenyl ketone (1173), 1-hydroxycyclohexyl-phenyl ketone (184), 2-methyl-1-{(4-methylthio)phenyl}-2-morpholinyl-1-propanone (907), 2,4,6-trimethylbenzoylbenzene-diphenylphosphine oxide (TPO), di(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (819), and 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-1-butanone (369).
[0029] Preferably, the anti-glare particles are hydrophobic and oleophilic micron-sized inorganic silica particles with an average particle size of 1.7 to 2.4 um, preferably 2.2 um. The anti-glare particles mainly provide haze and anti-glare effects, and the haze of the hardened layer can be controlled according to the amount of the anti-glare particles added.
[0030] Preferably, the hardened particles are solvent-based nano-scale inorganic silica particles with an average particle size of 15 to 70 nm, preferably 40 nm. The hardened particles mainly provide an effect of increasing wear resistance. Appropriate addition will not only not affect the overall appearance and haze of the hardened layer, but also can enhance the wear resistance of the hardened layer and increase the hardness of the hardened layer to a certain extent.
[0031] The technical solution adopted by the present invention to solve the above-mentioned second technical problem is: a tape using the above-mentioned coating, characterized in that it includes a substrate layer, a hardening layer and an adhesive layer, the hardening layer is coated on the front side of the substrate layer, the adhesive layer is coated on the back side of the substrate layer, and the hardening layer is formed by curing the coating described in claim 1.
[0032] The adhesive layer is OCA glue, which is a self-made adhesive produced by Ningbo Zongyan Chemical, and the thickness of the adhesive layer is 25um.
[0033] The substrate layer is selected from one of PET (polyethylene terephthalate), TAC (triacetyl cellulose), PI (polyimide), PEN (polyethylene naphthalate), PMMA (polymethyl methacrylate), and PC (polycarbonate), preferably a TAC substrate with high transmittance performance, and the thickness of the TAC substrate is preferably 60 to 100 um.
[0034] The adhesive tape provided by the present invention preferably has a haze range of about 4 to 15%, so as to ensure that it can provide a certain anti-glare performance in the actual application of the vehicle-mounted central control display external screen, while not affecting the overall clarity and brightness of the display screen. When the haze is lower than 4%, the adhesive tape cannot provide sufficient anti-glare effect; when the haze is greater than 15%, the display screen will be whitish as a whole, while reducing clarity and brightness.
[0035] The technical solution adopted by the present invention to solve the third technical problem is: a method for preparing the above-mentioned adhesive tape, characterized in that it comprises the following steps:
[0036] (1) adding the components of the coating in proportion and mixing them evenly, then coating the coating on the front side of the substrate layer, drying the coating, and UV curing the coating to form a hardened layer on the front side of the substrate layer;
[0037] (2) The adhesive layer is coated on the back side of the substrate layer and dried to obtain the adhesive tape.
[0038] The adhesive tape preparation method provided by the present invention has obvious cost advantages and a simple manufacturing process. The prepared hardened layer has high hardness and high wear resistance on the TAC substrate and can provide an excellent anti-fouling membrane surface effect.
[0039] The technical solution adopted by the present invention to solve the fourth technical problem is: an application of the above-mentioned tape, characterized in that the tape is used to be pasted on the surface of an electronic display screen.
[0040] Compared with the prior art, the advantages of the present invention are as follows: the anti-fouling and anti-glare coating provided by the present invention has excellent anti-fouling effect, and its basic principle is: a hexafunctional fluorine-containing silicon-specific modified acrylate oligomer is selected to be matched with two trifunctional and hexafunctional acrylate monomers, respectively; after UV radiation, the acrylic double bonds of the oligomer and the monomer will open and quickly bond with each other through free radical reactions to form a new cross-linked network structure, and the fluorine-silicon structure at the end of the side chain of the hexafunctional fluorine-containing silicon-specific modified acrylate oligomer will migrate to the surface of the cross-linked network structure due to its incompatibility with the main chain resin (here, it is distinguished from "fluorine-silicon elements are enriched to the surface" in the comparative literature, but "fluorine-silicon segments migrate to the surface due to compatibility"), forming a nano-microscopic rough structure; finally, since the fluorine-silicon segments are treated by grafting modification, the fluorine-silicon segments can be anchored in the cross-linked network, and the anti-fouling effect and weather resistance are stronger (compared with the "fluorine-silicon elements are enriched to the surface without outstanding weather resistance" in the comparative literature), just like the nanofiber structure on the surface of lotus leaves, which makes it difficult for water droplets or oil droplets to be wetted. The two multifunctional acrylate monomers not only enhance the cross-linking reaction activity, but also become part of the dense cross-linking network structure, just like large and small bricks embedded in a stone wall by volume, thereby enhancing the surface strength of the coating and improving its wear resistance and hardness properties.
[0041] From the above, it can be seen that the anti-fouling and anti-glare coating uses multi-functional fluorinated silicon-containing special modified acrylate oligomers to provide anti-fouling effects. The two multi-functional acrylate monomers and fluorinated silicon oligomers jointly construct a cross-linked network structure to enhance the surface strength of the film surface. Micron-level silica provides haze and anti-glare effects. Nano-level silica particles serve as surface performance enhancing particles, which can ensure excellent anti-fouling, hardness and wear resistance under a certain haze. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic structural diagram of the adhesive tape of the present invention. DETAILED DESCRIPTION
[0043] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0044] The chemical reagents used in the following examples and comparative examples can all be obtained from commercial channels. Unless otherwise specified, the following hexafunctional fluorine-containing silicon-containing special modified acrylate oligomer is a product of model FSP8638 purchased from Guangzhou Runao Chemical Co., Ltd., a hexafunctional acrylate monomer is a product of model FSP899 purchased from Sartomer Co., Ltd. of the United States, a trifunctional acrylate monomer is a product of model EM231 purchased from Changxing Materials Co., Ltd. of Taiwan, China, a photoinitiator is a product of model IGM907 purchased from Agenmon of the Netherlands, a leveling agent is a product of model EFKA3030 purchased from Efka of Germany, an anti-glare particle is a product of model SPB100 purchased from Fuji Silicon Chemical Co., Ltd. of Japan, and a hardened particle is a product of model C764 purchased from Evonik Chemical Co., Ltd. of Germany.
[0045] The anti-glare particles are all hydrophobic and oleophilic micron-sized inorganic silica particles, and the hardened particles are all solvent-based nano-sized inorganic silica particles.
[0046] The adhesive layers in the following embodiments are all OCA adhesive layers, which are self-made adhesives produced by Bosoken Chemical, with a model number of NC-838.
[0047] Example 1
[0048] The invention provides a stain-resistant anti-glare tape, which comprises a substrate layer, a hardening layer and an adhesive layer. The hardening layer is coated on the front side of the substrate layer, the adhesive layer is coated on the back side of the substrate layer, and the hardening layer is formed by curing the following coating. Figure 1 The reference numeral 1 refers to the adhesive layer; the reference numeral 2 refers to the substrate layer; and the reference numeral 3 refers to the hardening layer. The substrate layer is preferably a TAC substrate with high transmittance performance, and the thickness is preferably 60 to 100 μm.
[0049] The preparation method of the tape is:
[0050] (1) The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then the coating is evenly coated on the front side of the 60 μm thick TAC substrate layer by wire rod roller coating, and baked in a forced air drying oven at 80° C. for 3 minutes. After the coating surface is completely dried, UV curing is performed to form a 2-4 μm hardening layer on the front side of the substrate layer;
[0051] The UV curing energy of the hardened layer is 200-500 mJ / cm 2 ; UV curing light intensity of hard layer is 200~300mW / cm 2 .
[0052] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.9% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 8.8% of hexafunctional acrylate monomer, 3.5% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0053] (2) The adhesive layer can be uniformly coated on the back of the substrate layer by slit coating or the like, and then dried by infrared baking to obtain the adhesive tape.
[0054] Example 2
[0055] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0056] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 27.5% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 5.5% of hexafunctional acrylate monomer, 2.2% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0057] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0058] Example 3
[0059] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0060] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 18.3% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 12.1% of hexafunctional acrylate monomer, 4.8% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0061] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0062] Example 4
[0063] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0064] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.9% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 6.2% of hexafunctional acrylate monomer, 6.2% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0065] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0066] Example 5
[0067] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0068] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 19.4% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 7.5% of hexafunctional acrylate monomer, 3.0% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 22.9% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0069] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0070] Example 6
[0071] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0072] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 26.3% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 10.1% of hexafunctional acrylate monomer, 4.1% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 12.3% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0073] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0074] Comparative Example 1
[0075] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0076] The anti-fouling anti-glare coating is obtained by fully stirring and uniformly mixing 27.8% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 10.7% of hexafunctional acrylate monomer, 4.3% of trifunctional acrylate monomer, 2.1% of photoinitiator, 0.2% of leveling agent, 2.4% of anti-glare particles, and 52.5% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0077] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0078] Comparative Example 2
[0079] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0080] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.9% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 12.3% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0081] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0082] Comparative Example 3
[0083] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0084] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.9% of hexafunctional fluorine-containing silicon special modified acrylate oligomer, 12.3% of hexafunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0085] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0086] Comparative Example 4
[0087] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0088] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.9% of tri-functional fluorinated silicon-containing special modified acrylate oligomer (product of Guangzhou Runao Chemical Company with model FSP8668), 8.8% of hexa-functional acrylate monomer, 3.5% of tri-functional acrylate monomer (China Taiwan Changxing Materials), 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles (Japan Fuji Silicon Chemical Co., Ltd.), 17.6% of hardened particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly according to a mass ratio of 3:2). The content of the above materials is weight percentage.
[0089] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0090] Comparative Example 5
[0091] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0092] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.9% of hexafunctional aliphatic polyurethane acrylate oligomer (KOG-6511 purchased from Suzhou Naimukai Company), 8.8% of hexafunctional acrylate monomer, 3.5% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 2.0% of anti-glare particles, 17.6% of hardening particles, and 43.2% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly according to a mass ratio of 3:2). The content of the above materials is weight percentage.
[0093] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0094] Comparative Example 6
[0095] For the anti-fouling and anti-glare tape provided in Example 1, the preparation method of the hardened layer is as follows:
[0096] The anti-fouling anti-glare coating is obtained by fully stirring and mixing 22.7% of hexafunctional aliphatic polyurethane acrylate oligomer (PU664 purchased from Migen Special Chemical Co., Ltd., Japan), 8.7% of hexafunctional acrylate monomer, 3.5% of trifunctional acrylate monomer, 1.8% of photoinitiator, 0.2% of leveling agent, 0.7% of AF auxiliary agent (KY1203 purchased from Shin-Etsu Chemical, Japan), 2.0% of anti-glare particles, 17.5% of hardening particles, and 42.9% of organic solvent (including methyl isobutyl ketone and propylene glycol methyl ether, which are mixed uniformly in a mass ratio of 3:2). The content of the above materials is weight percentage.
[0097] The components of the anti-fouling and anti-glare coating are added in proportion and mixed evenly, and then can be evenly coated on the front side of the 60um thick TAC substrate layer by wire rod roller coating, baked in a blast drying oven at 80°C for 3 minutes, and after the coating surface is completely dry, UV curing is performed to form a 2-4um hardened layer on the front side of the substrate layer.
[0098] The main properties of the adhesive tapes provided in the embodiments and comparative examples of the present invention are tested using the following test methods / equipment and standards.
[0099] ⑴ Full light transmission: The equipment used is Japan Murakami Color Haze Meter, using D65 light source, and the test standard is JISK7361;
[0100] (2) Coating haze: The equipment used is Japanese Murakami color haze meter, using D65 light source, and the test standard is JIS K7136;
[0101] ⑶Thickness: Use Japanese Nikon altimeter display, the test error is 0.001mm;
[0102] ⑷ Pencil hardness: Use a handheld pencil hardness tester with a load of 750g, Mitsubishi special hardness test pencil, and the test standard is JIS K5600;
[0103] ⑸ Scratch resistance: Use the American TABER abrasion tester and Japanese TOKYUHANDS steel wool #0000 for 10 cycles back and forth for wear resistance test. The diameter of the friction head is R = 10mm. The wear resistance of the hardened layer is determined by detecting whether there are scratches on the surface of the diaphragm.
[0104] ⑹Glossiness: Use the equipment Xinjia multi-angle gloss meter, the test angle is 60°, and the test standard is JIS Z8741;
[0105] ⑺ Water contact angle / oil contact angle: The contact angle between the hardened surface of the hardened layer and deionized water and oleic acid was tested using the OCA15EC automatic contact angle measuring device manufactured by Eiko Seiki Co., Ltd.;
[0106] ⑻ Adhesion: Use the 100-grid method to test, using 3M 600 test tape, and determine the adhesion performance of the hardened layer by detecting whether the coating on the surface of the diaphragm has fallen off;
[0107] The adhesive tapes prepared in the above-mentioned embodiments and comparative examples can be used for sticking on the surface of an electronic display screen.
[0108] Schedule
[0109]
[0110]
[0111] The above-mentioned fluorine-modified oligomer refers to the hexafunctional fluorine-containing silicon-specific modified acrylate oligomer or the hexafunctional aliphatic polyurethane acrylate oligomer or the trifunctional fluorine-containing silicon-specific modified acrylate oligomer of the corresponding embodiment or comparative example; the hexafunctional reactive monomer refers to a hexafunctional acrylate monomer, and the trifunctional reactive monomer refers to a trifunctional acrylate monomer.
[0112] From the data in the above table, it can be seen that by comparing Examples 1, 2, 3 and Comparative Example 5, it can be seen that the finger-stain resistance of the tape is mainly provided by the fluorine-containing silicon-modified special acrylate oligomer, and the amount of the fluorine-containing silicon-modified special acrylate oligomer used determines the water contact angle and the oil contact angle of the coating, thereby affecting the surface tension of the hardened layer; by comparing Example 1 and Comparative Example 4, it can be seen that the functionality of the fluorine-containing silicon-modified special acrylate oligomer affects the surface strength of the hardened layer, including hardness and scratch resistance, but the difference in water contact angle and oil contact angle is small; by comparing Example 1 and Comparative Example 6, it can be seen that adding AF additives to non-fluorine-containing silicon-modified acrylate can make the coating have better finger-stain resistance, but AF additives are expensive and have harsh storage conditions, which is cost-effective. The surface is lower than that of using fluorine-containing silicon special modified acrylate oligomers; by comparing Examples 1, 4 with Comparative Examples 2, 3, it can be seen that the presence of multifunctional acrylate monomers can not only reduce the viscosity of the system but also participate in the curing reaction, and can also cross-link with the oligomers to form bonds, thereby improving the surface hardness and scratch resistance of the hardened layer. The functionality of the multifunctional acrylate monomer affects the surface strength of the final hardened layer. In addition, the use of a variety of multifunctional acrylate monomers can effectively improve the photocuring reaction activity of the anti-fouling and anti-glare coating; by comparing Examples 1, 5, 6 with Comparative Example 1, it can be seen that the hardening particles play a major role in the hardness and wear resistance of the hardened layer. The addition of nano-scale silica particles can significantly improve the surface strength of the hardened layer, but excessive addition will lead to a rapid increase in material costs.
[0113] The anti-fouling and anti-glare tape provided by the present invention has a hard layer made of hexafunctional fluorine-containing silicon special modified acrylate as the main resin, and is matched with two multifunctional acrylate monomers, so that the hard layer not only has a finger-stain resistance effect, but also has a higher surface reliability performance; in addition, micron-level silicon dioxide is used to provide haze and anti-glare effects, and nano-level silicon dioxide particles are used as surface performance enhancing particles to ensure that the hardness and wear resistance of the coating are further enhanced under a certain haze, so that the entire hard layer coating still exhibits excellent surface hardness and friction resistance when the dry film thickness is only 2 to 4 um.
[0114] The anti-glare hardened layer provided by the present invention has high hardness, high wear resistance and finger stain resistance effects at a relatively thin coating thickness, adopts a wet coating process, and has a relatively low cost.
[0115] The above is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. All equivalent changes and modifications made based on the content of the present invention are included in the patent scope of the present invention.
Claims
1. A stain-resistant anti-glare coating, characterized in that: The composition comprises the following weight percentages: Hexafunctional fluorine-containing silicone-modified acrylate oligomer 18.3-27.8%; Hexafunctional acrylate monomer 5.5-12.3%; Trifunctional acrylate monomer 2.2-12.3%; Photoinitiator 1.5-2.5%; Leveling agent 0.1~0.3%; Anti-glare particles 2.0% to 2.5%; Hardened particles 12.3-22.9%; Organic solvent 42.9%~52.5%.
2. The anti-fouling and anti-glare coating according to claim 2, characterized in that: The composition comprises the following weight percentages: Hexafunctional fluorine-containing silicon-modified special acrylate oligomer 22.9%; Hexafunctional acrylate monomer 8.8%; Trifunctional acrylate monomer 3.5%; Photoinitiator 1.8%; Leveling agent 0.15%; Anti-glare particles 2.0%; Hardened particles 17.6%; Organic solvent 43.3%.
3. The anti-fouling and anti-glare coating according to claim 1 or 2, characterized in that: The organic solvent includes methyl isobutyl ketone and propylene glycol methyl ether.
4. The anti-fouling and anti-glare coating according to claim 1 or 2, characterized in that: The leveling aid is EFKA3030, including polyether modified siloxane; The photoinitiator is one or more combinations of 2-hydroxy-2-methyl-1-phenyl ketone (1173), 1-hydroxycyclohexyl-phenyl ketone (184), 2-methyl-1-{(4-methylthio)phenyl}-2-morpholinyl-1-propanone (907), 2,4,6-trimethylbenzoylbenzene-diphenylphosphine oxide (TPO), di(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (819), and 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-1-butanone (369).
5. The anti-fouling and anti-glare coating according to claim 1 or 2, characterized in that: The anti-glare particles are hydrophobic and oleophilic micron-sized inorganic silica particles with an average particle size of 1.7 to 2.4 μm.
6. The anti-fouling and anti-glare coating according to claim 1 or 2, characterized in that: The hardened particles are solvent-based nanometer-scale inorganic silicon dioxide particles with an average particle size of 15 to 70 nm.
7. An adhesive tape using the coating according to any one of claims 1 to 6, characterized in that: It comprises a substrate layer, a hardening layer and an adhesive layer, wherein the hardening layer is coated on the front side of the substrate layer, the adhesive layer is coated on the back side of the substrate layer, and the hardening layer is formed by curing the coating according to claim 1.
8. A method for preparing the adhesive tape according to claim 7, characterized in that: The steps include: (1) adding the components of the coating in proportion and mixing them evenly, then coating the coating on the front side of the substrate layer, drying the coating, and UV curing the coating to form a hardened layer on the front side of the substrate layer; (2) The adhesive layer is coated on the back side of the substrate layer and dried to obtain the adhesive tape.
9. An application of the adhesive tape according to claim 7, characterized in that: The adhesive tape is used to be adhered to the surface of an electronic display screen.
Citation Information
Patent Citations
Non-glare coating and non-glare membrane
CN105566963A
Antifouling and anti-glare paint and preparation method thereof
CN111826061A
Anti-glare antireflection film for display
CN115508920A
Anti-glare Anti-reflection film for display
WO2024082511A1