Washable anticorrosive material and preparation method thereof
By optimizing the emulsifier structure, washable anticorrosion materials are prepared, which solves the problems of difficult to wash and remove existing temporary anticorrosion materials and is flammable and explosive, and achieves efficient anti-salt spray corrosion and ultraviolet aging performance to ensure that It has a safe and environmentally friendly protective effect.
Patent Information
- Application Number
- CN202411201615.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
AI Technical Summary
Existing temporary anticorrosion materials are difficult to wash and remove after construction, and contain flammable and explosive solvents. They have potential quality risks to the automotive paint surface and tires, and cannot effectively protect special-shaped parts and joints.
Non-ionic emulsifiers such as fatty alcohol polyoxyethylene ether and fatty amine polyoxyethylene ether are used to optimize the emulsifier structure to form an emulsification effect of oil-in-water and water-in-oil emulsification effect, and washable anticorrosion materials can be prepared. After coating, 80℃ can be used. The above hot water is quickly removed and does not contain solvents, providing good anti-salt spray corrosion and ultraviolet aging properties.
It realizes rapid water washing and removal of anticorrosive materials, avoids the risk of flammability and explosiveness, provides 200 hours of ultraviolet aging resistance and 480 hours of neutral salt spray corrosion resistance, and is safe and environmentally friendly.
Smart Images

Figure CN118931389A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of protective coatings, and in particular relates to a water-washable anticorrosive material and a preparation method thereof. Background Art
[0002] Common ocean-going cargoes include containers, complete vehicles, and large metal parts. They often take several months to transport and are always in a heavy salt spray environment. This heavy salt spray environment has a great corrosive impact on the damaged corners of the container, the exposed parts of the vehicle, and the paint surface of the vehicle body. In addition, the exposed paint surface is also subject to corrosion such as aging by ultraviolet rays. Therefore, temporary anti-corrosion materials are usually sprayed on the cargo before transportation.
[0003] The currently used temporary protective materials usually include tearable polyolefin films, solvent-based temporary anti-corrosion materials, and reactive cross-linked temporary protective coatings similar to varnish. Tearable polyolefin films are only used on flat parts and cannot cover special-shaped parts, corners, and gaps; solvent-based temporary anti-corrosion materials usually use volatile solvents such as kerosene and other alkanes as solvents, which have low flash points, are flammable and explosive during construction, and have potential quality risks to automobile paint, tire rubber and other parts; the anti-corrosion layer formed after the material is constructed also needs to be cleaned with kerosene and other solvents after reaching the client. The entire cleaning process is complicated and time-consuming. For example, water-washable wax needs to be applied with gasoline and wait for 10 minutes before being rinsed with high-pressure water.
[0004] Therefore, in view of the above technical problems, it is necessary to provide a water-washable anti-corrosion material and a preparation method.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0006] The object of the present invention is to provide a water-washable antiseptic material and a preparation method thereof.
[0007] In order to achieve the above object, a technical solution provided by a specific embodiment of the present invention is as follows:
[0008] The washable anticorrosive material comprises, by weight: 12-19% wax, 4-9% rust inhibitor, 4-13% resin emulsion, 7-15% nonionic emulsifier, 1-8% ultraviolet absorber, and the balance of deionized water, wherein the nonionic emulsifier is selected from fatty alcohol polyoxyethylene ether RO (CH2CH2O) nH, wherein R is a C12-C15 alkyl group, and n is 4-18. This solution optimizes the structure of fatty alcohol polyoxyethylene ether and considers many aspects such as its EO number and carbon chain structure, so that the water-based group of the emulsifier in the anti-corrosion material emulsion system before use is in a structural form of the outer side wrapping the inner oily group (water-in-oil) to form a good emulsification effect, and after coating, the oily group of the emulsifier is in a structural form of the outer side wrapping the inner water-based group (oil-in-water), which can maintain the stability of the wax layer structure and maintain high protectiveness; and when washed with hot water at 80°C, the disintegration of the wax layer is promoted, and it has a certain emulsification and dispersion effect, so as to achieve rapid and complete water washing and removal from the product surface.
[0009] In one or more embodiments of the present invention, the nonionic emulsifier further comprises fatty amine polyoxyethylene ether R1N[(CH2CH2O)pH][(CH2CH2O)mH], wherein the sum of m and p is 1 to 20, and R1 is a C12-C15 alkyl group.
[0010] In one or more embodiments of the present invention, the nonionic emulsifier is obtained by mixing fatty alcohol polyoxyethylene ether and fatty amine polyoxyethylene ether in a mass ratio of (2-5):1.
[0011] In one or more embodiments of the present invention, the UV absorber is selected from butyl methoxybenzophenone methane, salicylates, benzophenones, benzotriazoles, substituted acrylonitriles, and triazines.
[0012] In one or more embodiments of the present invention, the wax is selected from microcrystalline wax, refined paraffin wax, and Fischer-Tropsch wax.
[0013] In one or more embodiments of the present invention, the refined paraffin is selected from fully refined paraffin 56#, 58#, and 60#.
[0014] In one or more embodiments of the present invention, the microcrystalline wax is selected from: 65#, 70#, 75#, 80# and 90#.
[0015] In one or more embodiments of the present invention, the Fischer-Tropsch wax is selected from Sasolwax5803 and Qihong oxidized Fischer-Tropsch wax F608A.
[0016] In one or more embodiments of the present invention, the resin emulsion is selected from: Dow HG100 acrylic emulsion, Guangzhou Tongdes 3EA0661Y alkyd emulsion, Shandong Tongxu Chemical XQS-100 styrene-butadiene emulsion, Jiangsu Fuqisen 3330 epoxy ester emulsion.
[0017] In one or more embodiments of the present invention, a method for preparing a washable antiseptic material comprises:
[0018] The wax and rust inhibitor are melted and mixed evenly at high temperature and stirred thoroughly. Then, non-ionic emulsifier and ultraviolet absorber are added in sequence and stirred continuously until fully mixed. Then, deionized water is added and stirred evenly. When the temperature drops to below 80°C, the resin emulsion is added and stirred thoroughly to make it emulsified evenly and then naturally cooled to room temperature.
[0019] In one or more embodiments of the present invention, melting at high temperature means heating to 90-95° C. to fully melt and mix.
[0020] In one or more embodiments of the present invention, the wax and the rust inhibitor are melted and mixed at a high temperature, and stirred evenly, with a stirring speed of 100-200RPM (here the main consideration is that the wax with a low melting point is less difficult to mix), and then the non-ionic emulsifier and the ultraviolet absorber are added in sequence and stirred until fully mixed, with a stirring speed of 300-500RPM (here the main consideration is the rapid dispersion of the emulsifier), and then deionized water is added and stirred (the stirring speed is 100-200RPM, here the main consideration is to fully mix with water and promote emulsification) and cooled to below 80°C, and then the resin emulsion is added and stirred well, with a stirring speed of no more than 200RPM (here the main consideration is that the viscosity of the resin emulsion is high and demulsification is prevented by high-speed stirring), so that it is emulsified evenly and naturally cooled to room temperature.
[0021] Compared with the prior art, the wax protective layer removal method of the present invention is simple. After the car docks and arrives at the client, it is directly rinsed with hot water above 80 degrees Celsius. Of course, the effect of washing with hot water above 80 degrees Celsius at a pressure of 5-6MPa is better. The anti-corrosion layer on the surface of the car can be quickly removed, and it has a good anti-salt spray corrosion effect, can withstand 200 hours of ultraviolet (band 290-390) aging test, and the product does not contain solvents, is safe, environmentally friendly, and has no flammable and explosive risks. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 This is a photo of the water washing effect of the wax-based anticorrosive material in one embodiment of the present invention;
[0024] Figure 2 This is a photograph of the wax-based anticorrosive material in one embodiment of the present invention after 480 hours of neutral salt spray test. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0026] The anti-corrosion materials including but not limited to the following embodiments can be prepared by melting wax and rust inhibitor at a high temperature of 90-95°C, mixing them evenly and stirring them fully at a stirring speed of 100-200RPM, then adding non-ionic emulsifier and ultraviolet absorber in sequence and continuing to stir until fully mixed at a stirring speed of 300-500RPM, and then adding deionized water and stirring (stirring speed of 100-200RPM) evenly and cooling to below 80°C, adding resin emulsion and stirring fully at a stirring speed of no more than 200RPM to make it emulsified evenly, and naturally cooling to room temperature.
[0027] Neutral Salt Spray Test (NSS: Neutral Salt Spray Test): GB / T10125-2021 "Artificial atmosphere corrosion test salt spray test".
[0028] Needle penetration test: The depth of a standard cone loaded with 150 grams sinking into a sample wax specimen kept at 25°C within 5 seconds, the unit is 1 / 10 mm.
[0029] Example 1
[0030] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 12%, rust inhibitor sodium petroleum sulfonate 4%, resin emulsion Dow HG100 acrylic emulsion 4%, non-ionic emulsifier CH3 (CH2) 11 The dosage of O(CH2CH2O)6H is 7%, the ultraviolet absorber butyl methoxybenzophenone methane is 1%, and the balance is deionized water, wherein the wax is 90# microcrystalline wax.
[0031] The preparation is to melt the wax and the rust inhibitor at a high temperature of 90°C, mix them evenly and stir them thoroughly at a stirring speed of 100RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are fully mixed at a stirring speed of 300RPM, and then add deionized water and stir (stirring speed of 100RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 80RPM to make it emulsified evenly, and naturally cool to room temperature.
[0032] After one spraying, the sample of this embodiment forms a soft wax layer about 5 μm thick on the surface, and the wax layer has a needle penetration of 252; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 20S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5MPa for 5S.
[0033] Example 2
[0034] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 16%, rust inhibitor sodium petroleum sulfonate 7%, resin emulsion Dow HG100 acrylic emulsion 8.5%, non-ionic emulsifier CH3 (CH2) 11 The dosage of O(CH2CH2O)6H is 10%, the ultraviolet absorber butyl methoxybenzophenone methane is 3%, and the balance is deionized water, wherein the wax is refined paraffin wax 58#.
[0035] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 150RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 400RPM, and then add deionized water and stir (stirring speed of 150RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 120RPM to make it emulsified evenly, and naturally cool to room temperature.
[0036] After one spraying, the sample of this embodiment forms a soft wax layer about 5 μm thick on the surface, and the wax layer has a needle penetration of 254; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 20S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5MPa for 5S.
[0037] Example 3
[0038] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 19%, rust inhibitor sodium petroleum sulfonate 9%, resin emulsion Dow HG100 acrylic emulsion 13%, non-ionic emulsifier CH3 (CH2) 11 The dosage of O(CH2CH2O)6H is 15%, the ultraviolet absorber butyl methoxybenzophenone methane is 5%, and the balance is deionized water, wherein the wax is Fischer-Tropsch wax Sasolwax5803.
[0039] The preparation is to melt the wax and the rust inhibitor at a high temperature of 95°C, mix them evenly and stir them thoroughly at a stirring speed of 200RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are fully mixed at a stirring speed of 500RPM, and then add deionized water and stir (stirring speed of 200RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 200RPM to make it emulsified evenly, and naturally cool to room temperature.
[0040] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 253; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 20S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5MPa for 5S.
[0041] Example 4
[0042] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 The dosage of O(CH2CH2O)6H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0043] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0044] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 269; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed by direct rinsing with 80 degrees Celsius hot water for 40S without residue. Figure 1 As shown. Rinse with hot water at 80 degrees Celsius and 6.5 MPa for 5 seconds to completely remove the residue.
[0045] Example 5
[0046] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 The dosage of NH(CH2CH2O)6H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0047] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0048] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 260; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant bubbling and looseness, and has good adhesion to the surface of the test piece. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 20S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5MPa for 5S.
[0049] Example 6
[0050] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, CH3 (CH2) 11 The dosage of N[(CH2CH2O)6H]2 is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0051] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0052] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 262; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 35S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 6MPa for 5S.
[0053] Example 7
[0054] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 The dosage of N[(CH2CH2O)6H][(CH2CH2O)8H] is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0055] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0056] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 258; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. Directly rinse with 80 degrees Celsius hot water for 25S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5.5MPa for 5S to completely remove without residue.
[0057] Example 8
[0058] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 14The dosage of O(CH2CH2O)6H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0059] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0060] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a penetration of 255; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 35S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5.4MPa for 5S.
[0061] Example 9
[0062] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 14 O(CH2CH2O) 15 The amount of H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0063] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0064] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 252; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 35S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5.6MPa for 5S.
[0065] Example 10
[0066] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 14 O(CH2CH2O) 18 The amount of H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0067] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0068] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 250; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the test piece. Directly rinse with 80 degrees Celsius hot water for 35S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5.6MPa for 5S to completely remove without residue.
[0069] Embodiment 11
[0070] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 18The amount of H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0071] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0072] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 252; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 35S. It can be completely removed without residue by rinsing with the above hot water at 80 degrees Celsius at a pressure of 5.6MPa for 5S.
[0073] Example 12
[0074] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 NH[(CH2CH2O) 18 H] dosage is 12.3%, ultraviolet absorber phenyl salicylate is 1.75%, and deionized water is the balance, wherein the wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0075] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0076] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a penetration of 258; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. Directly rinse with 80 degrees Celsius hot water for 25S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5MPa for 5S to completely remove without residue.
[0077] Example 13
[0078] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 N[(CH2CH2O) 18 H][C2H5] is used in an amount of 12.3%, ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water, wherein the wax is Sasolwax5803.
[0079] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0080] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 257; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the test piece. Directly rinse with 80 degrees Celsius hot water for 25S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5.3MPa for 5S to completely remove without residue.
[0081] Embodiment 14
[0082] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 18H dosage is 12.3%, UV absorber phenyl salicylate is 1.75%, and the balance is deionized water, wherein the wax is fully refined paraffin wax 56#.
[0083] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0084] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 251; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. Directly rinse with 80 degrees Celsius hot water for 25S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5.4MPa for 5S to completely remove without residue.
[0085] Embodiment 15
[0086] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 18 H dosage is 12.3%, UV absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance Sasolwax5803.
[0087] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0088] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 250; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. Directly rinse with 80 degrees Celsius hot water for 25S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5.8MPa for 5S to completely remove without residue.
[0089] Example 16
[0090] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 18 H dosage is 12.3%, UV absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 56# fully refined paraffin wax.
[0091] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0092] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 250; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. Directly rinse with 80 degrees Celsius hot water for 30S to completely remove without residue. Rinse with the above hot water at 80 degrees Celsius at a pressure of 5.2MPa for 5S to completely remove without residue.
[0093] Embodiment 17
[0094] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 12The amount of H is 12.3%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0095] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0096] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 260; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 25S. It can be completely removed without residue by rinsing with hot water at 80 degrees Celsius at a pressure of 5.3MPa for 5S.
[0097] Embodiment 18
[0098] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 12 H dosage 9.84%, CH3(CH2) 11 The dosage of N[(CH2CH2O)6H]2 is 2.46%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0099] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0100] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 260; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 25S. It can be completely removed without residue by rinsing with hot water at 80 degrees Celsius at a pressure of 5.4MPa for 5S.
[0101] Embodiment 19
[0102] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O) 12 H dosage 10.24%, CH3(CH2) 11 The dosage of N[(CH2CH2O)6H]2 is 2.05%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0103] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0104] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 260; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 30S. It can be completely removed without residue by rinsing with hot water at 80 degrees Celsius at a pressure of 5.5MPa for 5S.
[0105] Embodiment 20
[0106] The raw materials of the washable anticorrosive material of this embodiment include, by weight: wax 13%, rust inhibitor lithium grease 8.13%, resin emulsion Jiangsu Fuqisen 3330 epoxy ester emulsion 6.25%, non-ionic emulsifier CH3 (CH2) 11 O(CH2CH2O)12 H dosage 8.2%, CH3(CH2) 11 The dosage of N[(CH2CH2O)6H]2 is 4.1%, the ultraviolet absorber phenyl salicylate is 1.75%, and the balance is deionized water. The wax is a mixture of 40% 65# microcrystalline wax and the balance 80# microcrystalline wax.
[0107] The preparation is to melt the wax and the rust inhibitor at a high temperature of 92°C, mix them evenly and stir them thoroughly at a stirring speed of 168RPM, then add the non-ionic emulsifier and the ultraviolet absorber in sequence and continue to stir until they are thoroughly mixed at a stirring speed of 370RPM, and then add deionized water and stir (stirring speed of 120RPM) evenly and cool to below 80°C, add the resin emulsion and stir thoroughly at a stirring speed of 180RPM to make it emulsified evenly, and naturally cool to room temperature.
[0108] After one spraying, the sample of this embodiment forms a 5μm thick soft wax layer on the surface, and the wax layer has a needle penetration of 260; it is resistant to neutral salt spray for 480 hours without corrosion. After 200 hours of UV (band 290-390, 200W, 1m distance irradiation) aging test, the wax layer thickness has no significant change, the surface has no significant blistering and looseness, and has good adhesion to the surface of the specimen. It can be completely removed without residue by directly rinsing with 80 degrees Celsius hot water for 28S. It can be completely removed without residue by rinsing with hot water at 80 degrees Celsius at a pressure of 5.6MPa for 5S.
[0109] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0110] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A washable antiseptic material, the raw materials of which include, by weight: wax 12-19%, rust inhibitor 4-9%, resin emulsion 4-13%, non-ionic emulsifier 7-15%, ultraviolet absorber 1-8%, and deionized water as the balance, wherein the non-ionic emulsifier includes fatty alcohol polyoxyethylene ether RO (CH2CH2O) n H, wherein R is a C12-C15 alkyl group, and n is 4-18.
2. The washable antiseptic material according to claim 1, characterized in that: The nonionic emulsifier also includes fatty amine polyoxyethylene ether R1N[(CH2CH2O)pH][(CH2CH2O)mH], wherein the sum of m and p is 1 to 20, and R1 is a C12-C15 alkyl group.
3. The washable antiseptic material according to claim 2, characterized in that: The nonionic emulsifier is obtained by mixing fatty alcohol polyoxyethylene ether and fatty amine polyoxyethylene ether in a mass ratio of (2-5):
1.
4. The washable antiseptic material according to claim 1, characterized in that: The ultraviolet absorber is selected from butyl methoxybenzophenone methane, salicylates, benzophenones, benzotriazoles, substituted acrylonitriles, and triazines.
5. The washable antiseptic material according to claim 1, characterized in that: The wax is selected from microcrystalline wax, refined paraffin wax and Fischer-Tropsch wax.
6. The washable antiseptic material according to claim 5, characterized in that: The refined paraffin is selected from fully refined paraffin 56#, 58#, and 60#.
7. The washable antiseptic material according to claim 5, characterized in that: The microcrystalline wax is selected from: 65#, 70#, 75#, 80# and 90#.
8. The washable antiseptic material according to claim 5, characterized in that: The Fischer-Tropsch wax is selected from Sasolwax5803 and Qihong oxidized Fischer-Tropsch wax F608A.
9. The washable antiseptic material according to claim 1, characterized in that: The resin emulsion is selected from: Dow HG100 acrylic emulsion, Guangzhou Tongdes 3EA0661Y alkyd emulsion, Shandong Tongxu Chemical XQS-100 styrene-butadiene emulsion, Jiangsu Fuqisen 3330 epoxy ester emulsion.
10. The method for preparing the washable antiseptic material according to any one of claims 1 to 9, comprising: The wax and rust inhibitor are melted and mixed evenly at high temperature and stirred thoroughly. Then, non-ionic emulsifier and ultraviolet absorber are added in sequence and stirred continuously until fully mixed. Then, deionized water is added and stirred evenly. When the temperature drops to below 80°C, the resin emulsion is added and stirred thoroughly to make it emulsified evenly and then naturally cooled to room temperature.
Citation Information
Patent Citations
Antirust emulsifying wax used for metal product
CN103342963A
Emulsifying wax composition, preparation method and applications thereof
CN106032436A
High solid content environmental-friendly anti-corrosion wax and preparation method thereof
CN106752949A
Water-based anticorrosive wax composition and application thereof
CN106800784A
Wax-containing composition for leather and its product surface coating
CN1611560A