Modulus control agent, low-modulus heat-conducting pressure-sensitive adhesive tape and preparation thereof
By combining the polycondensation products of hydroxyl-terminated polydimethylsiloxane and hydroxy MQ silicone resin with high thermal conductivity powder in thermal pressure-sensitive tape, an interpenetrating network structure is formed, and the contradiction between thermal conductivity and modulus is solved. It achieves high thermal conductivity, low modulus, and high temperature resistance tape, which improves the life and processing performance of components.
Patent Information
- Application Number
- CN202411201270.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When existing thermal pressure-sensitive tapes increase thermal conductivity, they lead to an increase in modulus, affecting the life of components, and have poor heat resistance, which cannot meet the needs of high-power components.
Using hydroxyl-terminated polydimethylsiloxane and hydroxy MQ silicone resin polycondensation products as modulus control agents to form an interpenetrating network structure, combining high-thermal conduction powders such as boron nitride and carbon nanotubes to reduce the thermal pressure-sensitive tape modulus and increase thermal conductivity.
Thermal pressure-sensitive tape with high thermal conductivity, low modulus, good bonding performance and excellent aging resistance is achieved, extending the life of the components and simplifying the manufacturing process.
Smart Images

Figure BDA0005017904260000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermal conductive adhesive tapes, and in particular to a modulus control agent, a method for preparing a low modulus thermal conductive pressure-sensitive adhesive tape using the modulus control agent, and the low modulus thermal conductive pressure-sensitive adhesive tape. Background Art
[0002] Thermally conductive tape is widely used in the design of heat-generating devices such as CPUs, power tubes, module power supplies, and screens because it has the functions of heat conduction and bonding. It also has the characteristics of softness, compressibility, conformability, and adaptability to a wide temperature range. With the rapid development of the electronics industry, electronic products tend to be lightweight, so the integration of electronic components is getting higher and higher. Under high operating frequencies, the heat generated by electronic components also increases rapidly. Heat dissipation capacity becomes the key to its lifespan. Therefore, the requirements for thermally conductive tape and its performance are increasing. At the same time, in the field of folding screens and under high-frequency vibration conditions, thermally conductive tape increases the thermal conductivity by increasing the amount of powder added, resulting in an increase in modulus and a decrease in component life.
[0003] The current method for preparing thermally conductive tapes is to add thermally conductive fillers to the colloid to achieve the purpose of thermal conductivity. However, the current thermally conductive pressure-sensitive tapes are mostly made of glass fiber as the base material, acrylic acid as the colloid, and compounded with thermally conductive powder. They have poor temperature resistance and a long-term use temperature of 100-125°C, which cannot meet the heat resistance requirements of high-power components. A small number of silicone-based thermally conductive tapes, such as CN102746799B, have the defects of low thermal conductivity, high cost, low bonding strength and high modulus. Therefore, how to control the modulus of the thermally conductive tape and provide a thermally conductive pressure-sensitive tape with high thermal conductivity, low modulus and high temperature resistance has become a technical problem that needs to be solved in this field. Summary of the invention
[0004] The purpose of the present invention is to provide a modulus controller, which comprises a hydroxyl-terminated polydimethylsiloxane and a hydroxyl MQ silicone resin condensation product. When the modulus controller is applied to a thermally conductive pressure-sensitive adhesive tape, it forms an interpenetrating network structure with the pressure-sensitive adhesive liquid, thereby increasing the resilience of the base adhesive and reducing the modulus of the thermally conductive pressure-sensitive adhesive tape. At the same time, the present invention provides a low-modulus thermally conductive pressure-sensitive adhesive tape and a preparation method thereof.
[0005] To this end, in one aspect of the present invention, a modulus control agent is provided, wherein the raw materials of the modulus control agent include: hydroxyl-terminated polydimethylsiloxane, hydroxyl MQ silicone resin, hydroxyl MQ silicone resin, an organic solvent and a condensation catalyst.
[0006] In a specific embodiment of the present invention, the raw materials of the modulus controller include, by weight: 100 parts of hydroxyl-terminated polydimethylsiloxane, 100-150 parts of hydroxyl MQ silicone resin, 50-300 parts of organic solvent, and 0.2-2 parts of condensation catalyst.
[0007] Preferably, the raw materials of the modulus controller include, by weight: 100 parts of hydroxyl-terminated polydimethylsiloxane, 110-130 parts of hydroxyl MQ silicone resin, 100-200 parts of organic solvent, and 0.5-1 part of condensation catalyst.
[0008] In a specific embodiment of the present invention, the viscosity of the hydroxyl-terminated polydimethylsiloxane is 50,000 to 1,000,000 mPa·s, preferably 400,000 to 800,000 mPa·s.
[0009] In a specific embodiment of the present invention, the hydroxyl content of the hydroxy MQ silicone resin is 2-5%, and the number average molecular weight is 3000-8000 g / mol. Preferably, the hydroxyl content of the hydroxy MQ silicone resin is 3-4%, and the number average molecular weight is 4000-6000 g / mol.
[0010] In a specific embodiment of the present invention, the organic solvent is one or more of toluene, xylene, ethyl acetate, and butyl acetate, preferably xylene.
[0011] In a specific embodiment of the present invention, the condensation catalyst is one or more of tetramethylammonium hydroxide, potassium hydroxide, dibutyltin dilaurate, and tetraisopropyl titanate, preferably dibutyltin dilaurate.
[0012] In the second aspect of the present invention, a method for preparing the above modulus controller is provided, comprising: mixing the raw materials of the modulus controller, then heating to 100-120° C., and stirring the reaction for 3-5 hours to obtain the modulus controller.
[0013] Specifically, the preparation method comprises: mixing hydroxyl-terminated polydimethylsiloxane, hydroxyl MQ silicone resin, organic solvent and catalyst in proportion, then heating to 100-120°C, stirring and reacting for 3-5 hours with water, and then cooling to room temperature to obtain the modulus controller, wherein the hydroxyl-terminated polydimethylsiloxane, hydroxyl MQ silicone resin, organic solvent and catalyst have the same meanings as described above.
[0014] In a third aspect of the present invention, there is provided a use of the above modulus control agent in a low modulus thermally conductive pressure-sensitive adhesive tape.
[0015] Specifically, by adding the above modulus controller to the raw materials of the thermally conductive pressure-sensitive adhesive tape, the modulus controller and the pressure-sensitive adhesive liquid form an interpenetrating network structure, which increases the resilience of the base adhesive and reduces the modulus of the thermally conductive pressure-sensitive adhesive tape without losing adhesion.
[0016] In a fourth aspect of the present invention, a low modulus thermally conductive pressure-sensitive adhesive tape is provided, wherein the raw material of the thermally conductive pressure-sensitive adhesive tape includes the modulus control agent as described above.
[0017] In a specific embodiment of the present invention, the raw materials of the thermally conductive pressure-sensitive adhesive tape include: vinyl methyl silicone rubber, methyl MQ resin, solvent, cross-linking agent, inhibitor, catalyst, modulus control agent as mentioned above, thermally conductive powder, and powder modifier.
[0018] In a specific embodiment of the present invention, the raw materials of the thermally conductive pressure-sensitive tape include, by weight: 100 parts of vinyl methyl silicone rubber, 120-200 parts of methyl MQ resin, 100-300 parts of solvent, 2-8 parts of cross-linking agent, 0.3-1.5 parts of inhibitor, 2-6 parts of platinum catalyst, 100-400 parts of modulus controller, 200-500 parts of thermal conductive powder, and 1-3 parts of powder modifier.
[0019] Preferably, the raw materials of the thermally conductive pressure-sensitive tape include: 100 parts of vinyl methyl silicone rubber, 140-180 parts of methyl MQ resin, 150-250 parts of solvent, 3-6 parts of cross-linking agent, 0.5-1 part of inhibitor, 3-5 parts of platinum catalyst, 150-300 parts of modulus controller, 300-400 parts of thermal conductive powder, and 1.5-2.5 parts of powder modifier.
[0020] In a specific embodiment of the present invention, the thermally conductive powder is one or more of aluminum oxide, aluminum nitride, boron nitride, silicon carbide, graphite, graphene and carbon nanotubes, preferably aluminum oxide, boron nitride and carbon nanotubes. Boron nitride and carbon nanotubes bridge with aluminum oxide powder to significantly improve the thermal conductivity of the material.
[0021] In a specific embodiment of the present invention, the powder modifier is one or more of methyltrimethoxysilane, vinyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, methyltriacetoxysilane, and vinyltriacetoxysilane, preferably hexadecyltrimethoxysilane.
[0022] In a specific embodiment of the present invention, the solvent is one or more of toluene, xylene, ethyl acetate, and butyl acetate, preferably xylene.
[0023] In a specific embodiment of the present invention, the crosslinking agent is hydrogen-containing silicone oil, and the hydrogen content is 0.4-1.6%, preferably 0.8-1.2%.
[0024] In a specific embodiment of the present invention, the inhibitor is ethynyl cyclohexanol.
[0025] In a specific embodiment of the present invention, the platinum content of the platinum catalyst is 2000-5000 ppm, preferably 3000-5000 ppm.
[0026] In a specific embodiment of the present invention, the vinyl content of the vinyl methyl silicone rubber is 0.01 to 0.15%, preferably 0.03 to 0.08%.
[0027] In a specific embodiment of the present invention, the molecular weight of the vinyl methyl silicone rubber is 300,000 to 800,000, preferably 450,000 to 650,000.
[0028] In a specific embodiment of the present invention, the M / Q ratio of the methyl MQ resin is 0.6 to 0.8, preferably 0.65 to 0.75.
[0029] In a specific embodiment of the present invention, the number average molecular weight of the methyl MQ resin is 3000-6000 g / mol, preferably 4000-5000 g / mol.
[0030] In a specific embodiment of the present invention, the hydroxyl content of the methyl MQ resin is 0.5-2%, preferably 0.8-1.2%.
[0031] In a fifth aspect of the present invention, a method for preparing the low modulus thermally conductive pressure-sensitive adhesive tape is provided, comprising:
[0032] Vinyl methyl silicone rubber, methyl MQ resin, solvent, cross-linking agent, inhibitor, modulus control agent, and powder modifier are mixed according to a certain proportion to obtain an organic silicone pressure-sensitive adhesive solution;
[0033] Adding thermally conductive powder into organic silicone pressure-sensitive adhesive liquid, adding platinum catalyst after modification, to obtain thermally conductive organic silicone pressure-sensitive adhesive;
[0034] The low modulus thermally conductive pressure-sensitive adhesive tape is obtained by coating a thermally conductive silicone pressure-sensitive adhesive on the surface of a substrate and performing a heating and curing treatment.
[0035] Wherein, the vinyl methyl silicone rubber, methyl MQ resin, solvent, cross-linking agent, inhibitor, modulus control agent, powder modifier, thermal conductive powder, and platinum catalyst have the meanings as described above.
[0036] In a specific embodiment of the present invention, the specific steps of the modification treatment include ball milling and ultrasonic treatment.
[0037] In a specific embodiment of the present invention, the specific steps of the heating and curing treatment include: first heating to 60-80°C, baking for 1-3 minutes, then heating to 120-150°C, and curing at this temperature for 3-5 minutes.
[0038] Beneficial effects:
[0039] (1) The modulus control agent provided by the present invention is a condensation product of hydroxyl-terminated polydimethylsiloxane and hydroxyl MQ silicone resin, which forms an interpenetrating network structure with the pressure-sensitive adhesive, increases the resilience of the base adhesive, and reduces the modulus of the thermally conductive pressure-sensitive adhesive tape without sacrificing adhesion.
[0040] (2) The present invention introduces high thermal conductivity powders of boron nitride and carbon nanotubes to bridge with alumina powder, thereby improving thermal conductivity while significantly reducing powder content, so that the modulus of the prepared thermally conductive pressure-sensitive adhesive tape is further reduced; by compounding the modulus control agent and the high thermal conductivity powder, a thermally conductive pressure-sensitive adhesive tape with high thermal conductivity, low modulus, good bonding performance, and excellent aging resistance is obtained, and at the same time, the tape is easy to manufacture and has good processing performance. DETAILED DESCRIPTION
[0041] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] The preparation method of the low modulus thermally conductive pressure-sensitive adhesive tape provided by the present invention comprises four steps: synthesis of a modulus control agent, preparation of an organic silicon pressure-sensitive adhesive solution, preparation of a thermally conductive organic silicon pressure-sensitive adhesive, and coating and curing, specifically:
[0043] Step 1, Synthesis of modulus control agent:
[0044] The hydroxyl-terminated polydimethylsiloxane, hydroxyl MQ silicone resin, organic solvent and catalyst are mixed, and then the temperature is raised to 100-120° C., water is separated and stirred for reaction for 3-5 hours, and the mixture is cooled to room temperature to obtain a modulus control agent.
[0045] in:
[0046] In parts by weight, 100 parts of hydroxyl-terminated polydimethylsiloxane; 100-150 parts of hydroxyl MQ silicone resin, preferably 110-130 parts; 50-300 parts of organic solvent, preferably 100-200 parts; 0.2-2 parts of condensation catalyst, preferably 0.5-1 part; the viscosity of the hydroxyl-terminated polydimethylsiloxane is 500,000-1,000,000 mPa·s, preferably 400,000-800,000 mPa·s;
[0047] The hydroxyl content of the hydroxy MQ silicone resin is 2-5%, preferably 3-4%; the number average molecular weight is 3000-8000 g / mol, preferably 4000-6000 g / mol;
[0048] The organic solvent is one or more of toluene, xylene, ethyl acetate, and butyl acetate, preferably xylene;
[0049] The condensation catalyst is one or more of tetramethylammonium hydroxide, potassium hydroxide, dibutyltin dilaurate, and tetraisopropyl titanate, preferably dibutyltin dilaurate.
[0050] Step 2: Preparation of silicone pressure-sensitive adhesive solution:
[0051] The vinyl methyl silicone rubber, methyl MQ resin, solvent, crosslinking agent, inhibitor, modulus control agent and powder modifier prepared in step 1 are uniformly mixed to obtain an organic silicone pressure-sensitive adhesive solution.
[0052] in:
[0053] In parts by weight, 100 parts of vinyl methyl silicone rubber; 120-200 parts of methyl MQ resin, preferably 140-180 parts; 100-300 parts of solvent, preferably 150-250 parts; 2-8 parts of cross-linking agent, preferably 3-6 parts; 0.3-1.5 parts of inhibitor, preferably 0.5-1 part; 100-400 parts of modulus control agent, preferably 150-300 parts; 1-3 parts of powder modifier, preferably 1.5-2.5 parts;
[0054] The vinyl content of the vinyl methyl silicone rubber is 0.01-0.15%, preferably 0.03-0.08%; the molecular weight is 300,000-800,000, preferably 450,000-650,000;
[0055] The M / Q ratio of the methyl MQ resin is 0.6 to 0.8, preferably 0.65 to 0.75; the number average molecular weight is 3000-6000 g / mol, preferably 4000 to 5000 g / mol; the hydroxyl content is 0.5 to 2%, preferably 0.8 to 1.2%;
[0056] The solvent is one or more of toluene, xylene, ethyl acetate, butyl acetate, etc., preferably xylene;
[0057] The cross-linking agent is hydrogen-containing silicone oil, with a hydrogen content of 0.4 to 1.6%, preferably 0.8 to 1.2%;
[0058] The inhibitor is ethynyl cyclohexanol;
[0059] The powder modifier is one or more of methyltrimethoxysilane, vinyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, methyltriacetoxysilane, and vinyltriacetoxysilane, preferably hexadecyltrimethoxysilane.
[0060] Step 3: Preparation of thermally conductive silicone pressure-sensitive adhesive:
[0061] The thermally conductive powder is added to the organic silicone pressure-sensitive adhesive solution prepared in step 2, and modified by ball milling and ultrasound. A platinum catalyst is added for mechanical mixing to prepare a thermally conductive organic silicone pressure-sensitive adhesive.
[0062] in:
[0063] The thermally conductive powder is one or more of aluminum oxide, aluminum nitride, boron nitride, silicon carbide, graphite, graphene and carbon nanotubes, preferably aluminum oxide, boron nitride and carbon nanotubes;
[0064] The platinum content of the platinum catalyst is 2000-5000 ppm, preferably 3000-5000 ppm;
[0065] In parts by weight, when the vinyl silicone rubber is 100 parts, the added amount of the platinum catalyst is 2 to 6 parts, preferably 3 to 5 parts; the added amount of the thermal conductive powder is 200 to 500 parts, preferably 300 to 400 parts.
[0066] Step 4: Coating and curing:
[0067] The thermally conductive silicone pressure-sensitive adhesive prepared in step 3 is coated on the surface of the substrate, first heated to 60-80°C, baked for 1-3 minutes, then heated to 120-150°C, and heat-cured for 3-5 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0068] The present invention is further described in detail below through specific examples.
[0069] Example 1
[0070] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 120g hydroxyl MQ silicone resin and 150g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein, the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa·s; the hydroxyl content of hydroxyl MQ silicone resin is 4% and the number average molecular weight is 4500g / mol.
[0071] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 17g of xylene and 15g of the above-mentioned modulus control agent are mixed and stirred evenly to obtain a silicone pressure-sensitive adhesive liquid; the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0072] Preparation of thermally conductive silicone pressure-sensitive adhesive: 19 g of boron nitride, 20 g of aluminum oxide, and 1 g of carbon nanotubes were added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was modified by ball milling at 600 rpm for 3 h, and then ultrasonicated for 30 min. After cooling to room temperature, 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0073] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0074] Example 2
[0075] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 120g hydroxyl MQ silicone resin and 150g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein, the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa·s; the hydroxyl content of hydroxyl MQ silicone resin is 4% and the number average molecular weight is 4500g / mol.
[0076] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 17g of xylene and 30g of the above-mentioned modulus control agent are mixed and stirred evenly to obtain an organosilicon pressure-sensitive adhesive liquid; wherein the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0077] Preparation of thermally conductive silicone pressure-sensitive adhesive: 19 g of boron nitride, 20 g of aluminum oxide, and 1 g of carbon nanotubes were added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was modified by ball milling at 600 rpm for 3 h, and then ultrasonicated for 30 min. After cooling to room temperature, 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0078] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0079] Example 3
[0080] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 120g hydroxyl MQ silicone resin and 150g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa·s; the hydroxyl content of hydroxyl MQ silicone resin is 4% and the number average molecular weight is 4500g / mol.
[0081] Preparation of organic silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 17g of xylene and 30g of the above-mentioned modulus control agent are mixed and stirred evenly to obtain an organic silicone pressure-sensitive adhesive liquid; wherein the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0082] Preparation of thermally conductive silicone pressure-sensitive adhesive: 70 g of aluminum oxide was added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was modified by ball milling at 600 rpm for 3 h, and then ultrasonicated for 30 min. After cooling to room temperature, 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive solution; the platinum content of the platinum catalyst was 4000 ppm.
[0083] Coating and curing: Coat the surface of the substrate with a thermally conductive silicone pressure-sensitive adhesive, then heat it to 80°C and bake it for 2 minutes, then heat it to 120°C and perform a heat-preservation and curing treatment for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and the low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0084] Example 4
[0085] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 140g hydroxyl MQ silicone resin and 160g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein, the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa·s; the hydroxyl content of hydroxyl MQ silicone resin is 3% and the number average molecular weight is 6000g / mol.
[0086] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 50g of xylene and 30g of the above-mentioned modulus control agent are mixed and stirred evenly to obtain a silicone pressure-sensitive adhesive liquid; the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0087] Preparation of thermally conductive silicone pressure-sensitive adhesive: 19 g of boron nitride, 20 g of aluminum oxide, and 1 g of carbon nanotubes were added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was modified by ball milling at 600 rpm for 3 h, and then ultrasonicated for 30 min. After cooling to room temperature, 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0088] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0089] Example 5
[0090] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 120g hydroxyl MQ silicone resin and 150g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein, the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa·s; the hydroxyl content of hydroxyl MQ silicone resin is 4% and the number average molecular weight is 4500g / mol.
[0091] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 18g of methyl MQ resin, 0.3g of hydrogenated silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 19g of xylene and 30g of the above-mentioned modulus control agent are mixed and stirred evenly to obtain a silicone pressure-sensitive adhesive liquid; the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogenated silicone oil is 1.2%.
[0092] Preparation of thermally conductive silicone pressure-sensitive adhesive: 19 g of boron nitride, 20 g of aluminum oxide, and 1 g of carbon nanotubes were added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was modified by ball milling at 600 rpm for 3 h, and then ultrasonicated for 30 min. After cooling to room temperature, 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0093] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0094] Comparative Example 1
[0095] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, and 17g of xylene are mixed and stirred evenly to obtain a silicone pressure-sensitive adhesive liquid; wherein the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0096] Preparation of thermally conductive silicone pressure-sensitive adhesive: 19 g of boron nitride, 20 g of aluminum oxide, and 1 g of carbon nanotubes were added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was modified by ball milling at 600 rpm for 3 h, and then ultrasonicated for 30 min. After cooling to room temperature, 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0097] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0098] Comparative Example 2
[0099] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 120g hydroxyl MQ silicone resin and 150g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein, the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa.s; the hydroxyl content of hydroxyl MQ silicone resin is 4% and the number average molecular weight is 4500g / mol.
[0100] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 17g of xylene and 50g of modulus control agent are mixed and stirred evenly to obtain an organosilicon pressure-sensitive adhesive liquid; the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0101] Preparation of thermally conductive silicone pressure-sensitive adhesive: 19 g of boron nitride, 20 g of aluminum oxide, and 1 g of carbon nanotubes were added to 100 g of the above-mentioned silicone pressure-sensitive adhesive solution, and the mixture was ball-milled at 600 rpm for 3 h, then ultrasonicated for 30 min, and then 0.6 g of platinum catalyst was added and mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0102] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0103] Comparative Example 3
[0104] Synthesis of modulus control agent: 100g hydroxyl-terminated polydimethylsiloxane, 120g hydroxyl MQ silicone resin and 150g xylene are mixed evenly; 1g dibutyltin dilaurate is added and mixed, then the temperature is raised to 120°C, water is separated and stirred for reaction for 4h, and the modulus control agent is obtained after cooling to room temperature; wherein, the viscosity of hydroxyl-terminated polydimethylsiloxane is 500,000 mPa.s; the hydroxyl content of hydroxyl MQ silicone resin is 4% and the number average molecular weight is 4500g / mol.
[0105] Preparation of silicone pressure-sensitive adhesive liquid: 10g of vinyl methyl silicone rubber, 15g of methyl MQ resin, 0.3g of hydrogen-containing silicone oil, 0.05g of ethynyl cyclohexanol, 0.25g of hexadecyltrimethoxysilane, 17g of xylene and 30g of the above-mentioned modulus control agent are mixed and stirred evenly to obtain an organosilicon pressure-sensitive adhesive liquid; the vinyl content of the vinyl methyl silicone rubber is 0.05% and the molecular weight is 600,000; the M / Q ratio of the methyl MQ resin is 0.68, the number average molecular weight is 5000g / mol, and the hydroxyl content is 1.1%; the hydrogen content of the hydrogen-containing silicone oil is 1.2%.
[0106] Preparation of thermally conductive silicone pressure-sensitive adhesive: 0.6 g of platinum catalyst was added to 100 g of the above silicone pressure-sensitive adhesive solution and the mixture was mechanically mixed to obtain a thermally conductive silicone pressure-sensitive adhesive; the platinum content of the platinum catalyst was 4000 ppm.
[0107] Coating and curing: the thermally conductive silicone pressure-sensitive adhesive is coated on the surface of the substrate, then heated to 80°C, baked for 2 minutes, and then heated to 120°C, and heat-insulated and cured for 4 minutes. The thermally conductive silicone pressure-sensitive adhesive is cured to form an adhesive layer, and a low modulus thermally conductive pressure-sensitive adhesive tape is obtained by lamination.
[0108] The test performance data of the thermally conductive silicone pressure-sensitive adhesives prepared in the above examples and comparative examples are shown in Table 1 below:
[0109] Table 1:
[0110]
[0111] As can be seen from the table, in the present invention, by introducing a self-made modulus control agent and a high thermal conductivity powder, the thermal conductivity of the thermally conductive pressure-sensitive adhesive tape is improved while the modulus is reduced, and the powder content is reduced. By compounding the two, a thermally conductive pressure-sensitive adhesive tape with high thermal conductivity, low modulus, good bonding performance, excellent aging resistance, convenient manufacturing, and good processing performance can be obtained.
[0112] In Comparative Example 1, no modulus control agent was added, resulting in a significant increase in the modulus of the product.
[0113] In Comparative Example 2, an excessive amount of modulus control agent was added, resulting in decreased adhesion and low cohesive strength of the product.
[0114] In Comparative Example 3, no thermal conductive powder was added, resulting in a decrease in the thermal conductivity of the product.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A modulus control agent, characterized in that The raw materials of the modulus control agent include: hydroxyl-terminated polydimethylsiloxane, hydroxyl MQ silicone resin, organic solvent and condensation catalyst.
2. The modulus control agent according to claim 1, characterized in that The raw materials of the modulus control agent include, by weight: 100 parts of hydroxyl-terminated polydimethylsiloxane, 100-150 parts of hydroxyl MQ silicone resin, 50-300 parts of organic solvent, and 0.2-2 parts of condensation catalyst; Preferably, the viscosity of the hydroxyl-terminated polydimethylsiloxane is 50,000 to 1,000,000 mPa·s, and the hydroxyl content of the hydroxyl MQ silicone resin is 2 to 5% and the number average molecular weight is 3,000 to 8,000 g / mol.
3. The modulus control agent according to claim 1, characterized in that The organic solvent is one or more of toluene, xylene, ethyl acetate, and butyl acetate; The condensation catalyst is one or more of tetramethylammonium hydroxide, potassium hydroxide, dibutyltin dilaurate, and tetraisopropyl titanate.
4. A method for preparing the modulus control agent according to any one of claims 1 to 3, characterized in that: include: The raw materials of the modulus control agent are mixed, and then the temperature is raised to 100-120° C., and the mixture is stirred for reaction for 3-5 hours to obtain the modulus control agent.
5. Use of the modulus control agent according to any one of claims 1 to 3 or obtained by the preparation method according to claim 4 in a low modulus thermally conductive pressure-sensitive adhesive tape.
6. A low modulus thermally conductive pressure-sensitive adhesive tape, characterized in that: The raw material of the thermally conductive pressure-sensitive adhesive tape includes the modulus control agent according to any one of claims 1 to 3.
7. The low modulus thermally conductive pressure-sensitive adhesive tape according to claim 6, characterized in that: The raw materials of the thermally conductive pressure-sensitive adhesive tape include, by weight: 100 parts of vinyl methyl silicone rubber, 120-200 parts of methyl MQ resin, 100-300 parts of solvent, 2-8 parts of cross-linking agent, 0.3-1.5 parts of inhibitor, 2-6 parts of platinum catalyst, 100-400 parts of modulus control agent, 200-500 parts of thermally conductive powder, and 1-3 parts of powder modifier; Preferably, the thermally conductive powder is one or more of aluminum oxide, aluminum nitride, boron nitride, silicon carbide, graphite, graphene and carbon nanotubes; Preferably, the powder modifier is one or more of methyltrimethoxysilane, vinyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, methyltriacetoxysilane, and vinyltriacetoxysilane; Preferably, the solvent is one or more of toluene, xylene, ethyl acetate, and butyl acetate; Preferably, the crosslinking agent is hydrogen-containing silicone oil, and the hydrogen content is 0.4-1.6%; Preferably, the inhibitor is ethynylcyclohexanol; Preferably, the platinum content of the platinum catalyst is 2000-5000 ppm.
8. The low modulus thermally conductive pressure-sensitive adhesive tape according to claim 6 or 7, characterized in that: The vinyl content of the vinyl methyl silicone rubber is 0.01-0.15% and the molecular weight is 300,000-800,000; Preferably, the M / Q ratio of the methyl MQ resin is 0.6-0.8, the number average molecular weight is 3000-6000 g / mol, and the hydroxyl content is 0.5-2%.
9. A method for preparing the low modulus thermally conductive pressure-sensitive adhesive tape according to any one of claims 6 to 8, characterized in that: include: Vinyl methyl silicone rubber, methyl MQ resin, solvent, cross-linking agent, inhibitor, modulus control agent, and powder modifier are mixed according to a certain proportion to obtain an organic silicone pressure-sensitive adhesive solution; Adding thermally conductive powder into organic silicone pressure-sensitive adhesive liquid, adding platinum catalyst after modification, to obtain thermally conductive organic silicone pressure-sensitive adhesive; The low modulus thermally conductive pressure-sensitive adhesive tape is obtained by coating a thermally conductive silicone pressure-sensitive adhesive on the surface of a substrate and performing a heating and curing treatment.
10. The preparation method according to claim 9, characterized in that: The specific steps of the modification treatment include ball milling and ultrasonic treatment; Preferably, the specific steps of the heating and curing treatment include: first heating to 60-80° C., baking for 1-3 minutes, then heating to 120-150° C., and curing at the temperature for 3-5 minutes.
Citation Information
Patent Citations
Self-adhesive organic silicon press-sensitive adhesive and preparation method thereof
CN104152104A
Preparation method of reworkable thermal conductive addition silicone rubber with low bonding strength and low splitting strength
CN109294240A
Organosilicon pressure-sensitive adhesive for hot-press lamination of silicone rubber as well as preparation method and application of organosilicon pressure-sensitive adhesive
CN117186830A
Non solvent silicone pressure sensitive adhesivecomposition
KR1020050069235A
Cited By
High-temperature-resistant organic silicon pressure-sensitive adhesive with high thermal conductivity as well as preparation method and application thereof
CN119799270A