Acrylate optical pressure-sensitive adhesive for OLED (Organic Light Emitting Diode) polarizer removal and preparation method of acrylate optical pressure-sensitive adhesive
By using acrylate optical pressure-sensitive adhesive in OLED display products, the problem of OLED brightness drop and inability to block low-band light waves in the prior art is solved, and high initial viscosity, peel force and UV absorption functions are realized to ensure the OLED screen Security and display effects.
Patent Information
- Application Number
- CN202410959158.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
AI Technical Summary
When existing OLED display products add polarizers to improve the display effect, their brightness decreases and cannot block low-band light waves, causing potential damage to the eyes. The market lacks effective optical pressure-sensitive adhesives to block ultraviolet-band light waves.
A kind of acrylate optical pressure-sensitive adhesive for OLED depolarizer, including acrylate resin, curing agent, UV absorber, UV-327 and blue light absorber, is used to form a high initial viscosity through specific ratios and preparation methods. , film with peeling force and UV aging resistance can absorb ultraviolet band light waves of 240 to 380 nm.
Without polarization, this film can effectively block the ultraviolet band light waves emitted by the OLED screen, prevent damage to the human eye, and maintain high initial viscosity and peeling force to ensure that the display effect is not affected.
Smart Images

Figure BDA0004949784790000061 
Figure BDA0004949784790000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of optical pressure-sensitive adhesives, in particular to an acrylate optical pressure-sensitive adhesive for an OLED depolarizer and a preparation method thereof. Background Art
[0002] As a newly emerged display unit, OLED is a self-luminous display without backlight and liquid crystal, with excellent color saturation, contrast and response speed. Because the material is lighter, thinner, transparent and flexible, OLED can achieve a variety of designs. The existing OLED needs to add a circular polarizer to improve the display effect due to the metal reflection of its own pixel points. After adding a polarizer to the display layer, the brightness of the OLED will drop sharply, but at the same time it blocks the damage to the eyes caused by low-band light waves (≤380nm). With the development of OLED technology, the technology of depolarizers has gradually been introduced into OLED display products, but this technology cannot block low-band light waves. Therefore, the market needs an optical pressure-sensitive adhesive to block low-band light waves. Summary of the invention
[0003] The purpose of the present invention is to provide an acrylate optical pressure-sensitive adhesive for an OLED depolarizer and a preparation method thereof in view of the deficiencies in the prior art. The acrylate optical pressure-sensitive adhesive for an OLED depolarizer has high initial adhesion and peeling strength, and at the same time has the functions of UV aging resistance and UV band (240-380nm) absorption, which can ensure that when the OLED screen is without a polarizer, the ultraviolet band emitted by the OLED will not enter the human eye and cause damage to the human eye.
[0004] In order to achieve the above technical objectives, the present invention adopts the following technical solutions.
[0005] The invention discloses an acrylate optical pressure-sensitive adhesive for an OLED depolarizer. The acrylate optical pressure-sensitive adhesive comprises the following components in parts by weight: 100 parts of acrylate resin; 0.1 to 1 part of curing agent; 0.1 to 0.4 parts of UV absorber UV-P; 0.1 to 0.4 parts of UV absorber UV-327; and 0.1 to 0.4 parts of blue light absorber BLA-1.
[0006] Specifically, the acrylic resin is polymerized from the following raw materials in parts by weight:
[0007] 60 parts of butyl acrylate, 80 parts of isooctyl acrylate, 30 parts of hydroxyethyl acrylate, 90 parts of tetrahydrofuran acrylate, 30 parts of cyclohexyl acrylate, 2 parts of initiator, and 350 parts of ethyl acetate.
[0008] The weight ratio of the acrylic resin to each absorbent is 100:0.1-0.4.
[0009] Preferably, the curing agent is N75 curing agent.
[0010] Preferably, the initiator is azobisisobutyronitrile.
[0011] A method for preparing the acrylic optical pressure-sensitive adhesive for the OLED depolarizer is further provided, comprising the following steps:
[0012] Step 1, add acrylate resin, curing agent, UV absorber UV-P, UV absorber UV-327, and blue light absorber BLA-1 into a container according to the ratio, stir and mix evenly to obtain a glue solution;
[0013] Step 2, filtering the obtained adhesive solution, placing the filtered adhesive solution into a vacuum degassing machine for degassing, taking it out after there are no bubbles inside the adhesive solution, and evenly coating it on the surface of the silicone release film with a scraper;
[0014] Step 3: Place the silicone release film coated with the adhesive in an oven for high-temperature drying and curing. After baking, take it out to obtain the acrylic optical pressure-sensitive adhesive, and use the silicone release film to adhere to the surface of the acrylic optical pressure-sensitive adhesive without release film.
[0015] Specifically, the preparation method of the acrylic resin in step 1 is as follows:
[0016] Step 11, add 36 parts of butyl acrylate, 54 parts of isooctyl acrylate, 18 parts of hydroxyethyl acrylate, 54 parts of tetrahydrofuran acrylate, 18 parts of cyclohexyl acrylate and 320 parts of ethyl acetate into a reactor, start stirring, and pass nitrogen into the reactor for 2 hours. After the nitrogen passing is completed, heat the reactor to 64°C;
[0017] Step 12, take 24 parts of butyl acrylate, 26 parts of isooctyl acrylate, 12 parts of hydroxyethyl acrylate, 36 parts of tetrahydrofuran acrylate, 12 parts of cyclohexyl acrylate, 30 parts of ethyl acetate, and 2 parts of initiator azobisisobutyronitrile, add them to the dropping kettle, start stirring and mixing, and pass nitrogen for 30 minutes. After the nitrogen is passed, the mixed solution in the dropping kettle is uniformly added dropwise to the reactor for 4 hours. During the dropping process, the temperature of the reactor is controlled to be maintained at 62-66°C;
[0018] Step 13: After the dropwise addition is completed, the reactor is heated to 68° C. and kept warm for 12 hours. After the heat preservation is completed, the reactor is cooled to room temperature to obtain an acrylate resin raw material.
[0019] Preferably, the filter medium in step 2 is a nylon filter with a filter mesh size of 500 meshes.
[0020] Preferably, the high temperature drying and curing in step 3 has a curing temperature of 95° C. and a curing time of 1 h.
[0021] The beneficial effects of the present invention are:
[0022] The acrylate optical pressure-sensitive adhesive for the OLED depolarizer of the present invention has high initial adhesion and peeling strength, and has the functions of UV aging resistance and UV band (240-380nm) absorption, which can ensure that when the OLED screen is without a polarizer, the ultraviolet band emitted by the OLED will not enter the human eye and cause damage to the human eye. DETAILED DESCRIPTION
[0023] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.
[0024] Example
[0025] The invention provides an acrylate optical pressure-sensitive adhesive for an OLED depolarizer, comprising the following components in parts by weight: 100 parts of acrylate resin; 0.1 parts of curing agent N75; 0.1 parts of UV absorber UV-P; 0.1-0.4 parts of UV absorber UV-327; and 0.1-0.4 parts of blue light absorber BLA-1.
[0026] Wherein, the acrylic resin is polymerized from the following raw materials in parts by weight:
[0027] 60 parts of butyl acrylate, 80 parts of isooctyl acrylate, 30 parts of hydroxyethyl acrylate, 90 parts of tetrahydrofuran acrylate, 30 parts of cyclohexyl acrylate, 2 parts of initiator azobisisobutyronitrile, and 350 parts of ethyl acetate.
[0028] The weight ratio of the acrylic resin to each absorbent is 100:0.1-0.4.
[0029] The preparation method of the acrylic resin is as follows:
[0030] 1) 36 parts of butyl acrylate, 54 parts of isooctyl acrylate, 18 parts of hydroxyethyl acrylate, 54 parts of tetrahydrofuran acrylate, 18 parts of cyclohexyl acrylate and 320 parts of ethyl acetate were added to a reactor, stirring was started, and nitrogen was passed through the reactor for 2 hours. After the nitrogen passing was completed, the reactor was heated to 64° C.;
[0031] 2) Take 24 parts of butyl acrylate, 26 parts of isooctyl acrylate, 12 parts of hydroxyethyl acrylate, 36 parts of tetrahydrofuran acrylate, 12 parts of cyclohexyl acrylate, 30 parts of ethyl acetate and 2 parts of initiator azobisisobutyronitrile, add them into the dropping kettle, stir and mix, and pass nitrogen for 30 minutes. After the nitrogen is passed, the mixed solution in the dropping kettle is uniformly added to the reactor. The dropping time is 4 hours. During the dropping process, the temperature of the reactor is controlled to be maintained at 62-66°C;
[0032] 3) After the addition is completed, the reactor is heated to 68° C. and kept warm for 12 hours. After the insulation is completed, the reactor is cooled to room temperature to obtain an acrylate resin raw material.
[0033] The method for preparing the acrylic optical pressure-sensitive adhesive for the OLED depolarizer described in this embodiment comprises the following steps:
[0034] Step 1, add acrylate resin, curing agent, UV absorber UV-P, UV absorber UV-327, and blue light absorber BLA-1 into a container according to the ratio, stir and mix evenly to obtain a glue solution;
[0035] Step 2, filtering the obtained glue solution, using a nylon filter medium with a filtration mesh of 500 mesh, placing the filtered glue solution into a vacuum degassing machine for degassing, taking it out after there are no bubbles inside the glue solution, and evenly coating it on the surface of the silicone release film with a scraper;
[0036] Step 3: Place the silicone release film coated with the adhesive in an oven for high-temperature drying and curing at 95°C for 1 hour. After baking, take out the film to obtain the acrylic optical pressure-sensitive adhesive, and use the silicone release film to adhere to the surface of the acrylic optical pressure-sensitive adhesive without release film.
[0037] Example 1
[0038] In this embodiment, 100 parts of acrylic resin, 0.1 parts of curing agent N75, and 0.1 parts of UV absorber UV-P are taken; the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles in the mixed liquid, take it out, use a scraper to apply it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0039] Example 2
[0040] In this embodiment, 120 parts of acrylic resin, 0.5 parts of curing agent N75, and 0.2 parts of UV absorber UV-P are taken, and the above raw materials are mixed evenly and filtered. After filtering, the mixture is put into a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, it is taken out and coated on the release surface of the release film with a scraper. After coating, it is put into an oven for drying and curing. The curing temperature is 95°C and the curing time is 60 minutes. After baking, it is taken out and covered with a release film for standby use.
[0041] Example 3
[0042] In this embodiment, 150 parts of acrylic resin, 51 parts of curing agent N7, and 0.4 parts of UV absorber UV-P are taken, and the above raw materials are mixed evenly and filtered. After filtering, the mixture is put into a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, it is taken out and coated on the release surface of the release film with a scraper. After coating, it is put into an oven for drying and curing. The curing temperature is 95°C and the curing time is 60 minutes. After baking, it is taken out and covered with a release film for standby use.
[0043] Example 4
[0044] In this embodiment, 200 parts of acrylic resin, 1 part of curing agent N75, and 0.4 part of UV absorber UV-P are taken, the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles in the mixed liquid, take it out, use a scraper to apply it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0045] Example 5
[0046] In this embodiment, 100 parts of acrylic resin, 0.1 parts of curing agent N75, and 0.1 parts of UV absorber UV-327 are taken, the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles in the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0047] Example 6
[0048] In this embodiment, 120 parts of acrylic resin, 0.5 parts of curing agent N75, and 0.2 parts of UV absorber UV-327 are taken, and the above raw materials are mixed evenly and filtered. After filtering, they are placed in a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0049] Example 7
[0050] In this embodiment, 150 parts of acrylic resin, 51 parts of curing agent N7, and 0.4 parts of UV absorber UV-327 are taken, and the above raw materials are mixed evenly and filtered. After filtering, they are placed in a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, and put it into an oven for drying and curing after coating. The curing temperature is 95°C and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0051] Example 8
[0052] In this embodiment, 200 parts of acrylic resin, 1 part of curing agent N75, and 0.4 parts of UV absorber UV-327 are taken, the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0053] Example 9
[0054] In this embodiment, 100 parts of acrylic resin, 0.1 parts of curing agent N75, and 0.1 parts of blue light absorber BLA-1 are taken, the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles in the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0055] Example 10
[0056] In this embodiment, 100 parts of acrylic resin, 0.1 parts of curing agent N75, 0.1 parts of UV absorber UV-P, 0.1 parts of UV absorber UV-327, and 0.1 parts of blue light absorber BLA-1 are taken, the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0057] Embodiment 11
[0058] In this embodiment, 100 parts of acrylic resin, 0.1 parts of curing agent N75, 0.2 parts of UV absorber UV-P, 0.2 parts of UV absorber UV-327, and 0.1 parts of blue light absorber BLA-1 are taken, and the above raw materials are mixed evenly and filtered. After filtering, the mixture is put into a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, it is taken out and coated on the release surface of the release film with a scraper. After coating, it is put into an oven for drying and curing. The curing temperature is 95°C and the curing time is 60 minutes. After baking, it is taken out and covered with a release film for standby use.
[0059] Example 12
[0060] In this embodiment, 100 parts of acrylic resin, 0.1 parts of curing agent N75, 0.4 parts of UV absorber UV-P, and 0.4 parts of UV absorber UV-327 are taken, the above raw materials are mixed evenly and filtered, and then put into a vacuum degassing machine for degassing. After there are no bubbles inside the mixed liquid, take it out, use a scraper to coat it on the release surface of the release film, put it into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. After baking, take it out, cover it with a release film, and set it aside.
[0061] Comparative Example
[0062] Take 100 parts of acrylic resin and 0.1 part of curing agent N75, mix the two evenly and filter them. After filtering, put them into a vacuum degassing machine for degassing. Take them out after there are no bubbles inside the mixed liquid, use a scraper to apply it on the release surface of the release film, put them into an oven for drying and curing after coating, the curing temperature is 95°C, and the curing time is 60 minutes. Take them out after baking, cover them with release film and set them aside.
[0063] The film samples prepared in the above Examples 1-10 and Comparative Examples were subjected to peeling force, holding force and optical tests, and the testing process is as follows.
[0064] 1) Peel force test
[0065] The film sample was cut into strips of 25 mm × 200 mm in size, and the surface of the stainless steel (SUS) was cleaned with ethanol and acetone. After cleaning, the light release film of the strip was torn off, and a 2 kg rubber roller was used to manually bond it to the surface of the SUS (Kejian KJ-6001A), rolling back and forth three times. After bonding, it was placed in a 23°C / 65%Rh environment for 20 min, 24 h, and 72 h, respectively. The 180° peeling force was tested at a speed of 300 mm / min using a universal testing machine, and the data was recorded. Five samples were tested for each condition, and the average value was taken.
[0066] 2) Adhesion test
[0067] Cut the film sample into a strip of 25mm×90mm in size, and use a 2Kg rubber roller to stick it to the steel plate for holding force test (Kejian KJ-6002A), with a bonding area of 25mm×25mm, and fix the steel plate with load weight on the other end. After bonding, leave it for 20 minutes, then hang the load weight, suspend it in the air, put it in a constant temperature oven for testing, and record the sliding distance or weight drop time.
[0068] 3) Optical test
[0069] The film sample was cut into pieces of 25 mm × 25 mm in size, the light film was removed, and the pieces were attached to the surface of optically transparent glass using a 2 kg rubber roller. The heavy release film was removed, and the pieces were placed in a UV spectrophotometer Cary700D for transmittance and Lab value determination.
[0070] The test results are shown in Table 1 below.
[0071] Table 1. Comparison of peel force, holding force and optical test results
[0072]
[0073]
[0074] It can be seen from the above table that the acrylic optical pressure-sensitive adhesive for OLED depolarizer provided by the present invention has the same initial adhesion and peeling force as traditional pressure-sensitive adhesives, and at the same time has the functions of UV aging resistance and UV band (240-380nm) absorption, which can ensure that when the OLED screen is without a polarizer, the ultraviolet band emitted by the OLED will not enter the human eye and cause damage to the human eye.
[0075] The preferred embodiments of the present invention are specifically described above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. An acrylic optical pressure-sensitive adhesive for an OLED depolarizer, characterized in that: The acrylic optical pressure-sensitive adhesive comprises the following components in parts by weight: 100 parts of acrylic resin; 0.1-1 parts of curing agent; 0.1-0.4 parts of UV absorber UV-P; 0.1-0.4 parts of UV absorber UV-327; Blue light absorber BLA-1 0.1~0.4 parts.
2. The acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 1, characterized in that: The acrylic resin is polymerized from the following raw materials in parts by weight: 60 parts of butyl acrylate, 80 parts of isooctyl acrylate, 30 parts of hydroxyethyl acrylate, 90 parts of tetrahydrofuran acrylate, 30 parts of cyclohexyl acrylate, 2 parts of initiator, and 350 parts of ethyl acetate.
3. The acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 1, characterized in that: The weight ratio of the acrylic resin to each absorbent is 100:0.1-0.
4.
4. The acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 1, characterized in that: The curing agent is N75 curing agent.
5. The acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 2, characterized in that: The initiator is azobisisobutyronitrile.
6. A method for preparing the acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claims 1-5, characterized in that: The following steps are involved: Step 1, add acrylate resin, curing agent, UV absorber UV-P, UV absorber UV-327, and blue light absorber BLA-1 into a container according to the ratio, stir and mix evenly to obtain a glue solution; Step 2, filtering the obtained adhesive solution, placing the filtered adhesive solution into a vacuum degassing machine for degassing, taking it out after there are no bubbles inside the adhesive solution, and evenly coating it on the surface of the silicone release film with a scraper; Step 3: Place the silicone release film coated with the adhesive in an oven for high-temperature drying and curing. After baking, take it out to obtain the acrylic optical pressure-sensitive adhesive, and use the silicone release film to adhere to the surface of the acrylic optical pressure-sensitive adhesive without release film.
7. The method for preparing the acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 6, characterized in that: The preparation method of the acrylic resin in step 1 is as follows: Step 11, add 36 parts of butyl acrylate, 54 parts of isooctyl acrylate, 18 parts of hydroxyethyl acrylate, 54 parts of tetrahydrofuran acrylate, 18 parts of cyclohexyl acrylate and 320 parts of ethyl acetate into a reactor, start stirring, and pass nitrogen into the reactor for 2 hours. After the nitrogen passing is completed, heat the reactor to 64°C; Step 12, take 24 parts of butyl acrylate, 26 parts of isooctyl acrylate, 12 parts of hydroxyethyl acrylate, 36 parts of tetrahydrofuran acrylate, 12 parts of cyclohexyl acrylate, 30 parts of ethyl acetate, and 2 parts of initiator azobisisobutyronitrile, add them to the dropping kettle, start stirring and mixing, and pass nitrogen for 30 minutes. After the nitrogen is passed, the mixed solution in the dropping kettle is uniformly added dropwise to the reactor for 4 hours. During the dropping process, the temperature of the reactor is controlled to be maintained at 62-66°C; Step 13: After the dropwise addition is completed, the reactor is heated to 68° C. and kept warm for 12 hours. After the heat preservation is completed, the reactor is cooled to room temperature to obtain an acrylate resin raw material.
8. The method for preparing the acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 6, characterized in that: The filter medium in step 2 is a nylon filter with a filter mesh size of 500 meshes.
9. The method for preparing the acrylic optical pressure-sensitive adhesive for OLED depolarizer according to claim 6, characterized in that: The high temperature drying and curing described in step 3 has a curing temperature of 95° C. and a curing time of 1 h.