Organic silicon heat-conducting adhesive and preparation method thereof

By using vinyl silicone oil, methyl MQ silicone resin and alumina fiber powder in organic silicone thermal glue, a thermal network structure is formed, which solves the problem of insufficient separation and mechanical properties of thermal powder, and achieves a higher Improved thermal conductivity and mechanical properties.

CN118931483APending Publication Date: 2024-11-12CHAMBROAD CHEM IND RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095193.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The thermally conductive powders of existing silicone thermal glues are easy to separate, settle and plate bond, and the tensile strength and bond strength are poor, which limits the stability and comprehensive performance of their application performance.

Method used

Vinyl silicone oil, methyl MQ silicone resin, hydrogen-containing silicone oil, alumina fibers and alumina powders are used as thermal fillers to form a thermal network path structure through the synergistic action of fibers and powders, and inhibitors and Caster catalysts are added. Control the addition reaction of silicon hydrogen to improve thermal conductivity and mechanical properties.

Benefits of technology

By forming a thermal conductivity network structure and a reinforced material interface, the thermal conductivity and mechanical properties of the silicone adhesive are improved, the separation and settlement of powder are reduced, and its heat resistance, heat dissipation, crack resistance and tensile properties are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of organosilicone heat-conducting adhesives, in particular to an organosilicone heat-conducting adhesive and a preparation method thereof. According to the adhesive, vinyl silicone oil is used as base adhesive, hydrogen-containing silicone oil is used as a cross-linking agent, methyl MQ silicon resin is used as a reinforcing agent, alumina fibers and alumina powder are used as heat-conducting fillers, and an inhibitor and a Karst catalyst are added at the same time to control a hydrosilylation reaction. Through the synergistic effect of the fibers and the powder, a heat-conducting network path structure is formed and becomes a fiber reinforced material, so that the heat-conducting property and the mechanical property of the organic silica gel adhesive are improved, and the phenomena of separation, sedimentation and hardening of the heat-conducting powder in the organic silica gel adhesive are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic silicon thermally conductive adhesives, in particular to an organic silicon thermally conductive adhesive and a preparation method thereof. Background Art

[0002] Silicone thermal conductive adhesive is based on organic silica gel, with thermal conductive fillers added. After a certain preparation process, it can obtain electronic grade potting adhesive, which has good thermal conductivity and electrical insulation properties, plays a role in ensuring the stability of electronic components during use and improving the performance of electronic products.

[0003] The thermal conductive filler in silicone thermal conductive adhesive is generally inorganic powder. Filling with a high proportion of inorganic powder can improve its thermal conductivity. The thermal conductive powder in silicone thermal conductive adhesive is generally in a loose accumulation state. As the storage time increases, the powder in the adhesive gradually separates, settles, and hardens, which is not conducive to the stability of the application performance of silicone adhesive.

[0004] In addition, the tensile strength of organic silicone adhesive is not high and the bonding strength is poor, which are the main factors that currently limit the application of organic silicone adhesive. Improving the heat resistance, heat dissipation, crack resistance, and tensile properties of organic silicone adhesive materials and preparing organic silicone thermal conductive adhesives with excellent comprehensive performance are the main development directions in the future. Summary of the invention

[0005] In view of the prior art, the present invention provides a silicone thermal conductive adhesive and a preparation method thereof. The adhesive uses vinyl silicone oil as a base adhesive, hydrogenated silicone oil as a crosslinking agent, methyl MQ silicone resin as a reinforcing agent, alumina fiber and alumina powder as thermal conductive fillers, and an inhibitor and a Custer catalyst are added to control the hydrosilylation reaction. Through the synergistic effect of the fiber and the powder, a thermal conductive network pathway structure is formed to become a fiber-reinforced material, which improves the thermal conductivity and mechanical properties of the silicone adhesive and reduces the separation, sedimentation, and compaction of the thermal conductive powder in the silicone adhesive.

[0006] The technical solution of the present invention includes:

[0007] A silicone thermally conductive adhesive, the components of which are measured by weight: 90-150 parts of vinyl silicone oil, 10-70 parts of methyl MQ silicone resin, 5-30 parts of hydrogen-containing silicone oil, 50-80 parts of thermally conductive filler, 0.1-1 part of inhibitor, and 0.1-2 parts of Custer catalyst. The thermally conductive filler is alumina fiber and alumina powder, and the mass ratio of fiber to powder is 1:3-1:9.

[0008] Preferably, the vinyl silicone oil is a branched vinyl silicone oil, a linear vinyl silicone oil, or a mixture of one or more linear and branched vinyl silicone oils; more preferably, its viscosity ranges from 1000 to 5000 mPa·s.

[0009] Preferably, the particle size of the methyl MQ silicone resin is in the range of 50 to 150 μm.

[0010] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 1 wt% to 1.45 wt%.

[0011] Preferably, the diameter of the alumina fiber is 5 to 10 μm, and the length is 10 to 50 μm; the average particle size of the alumina powder is 5 to 10 μm.

[0012] Preferably, the inhibitor is selected from one or two of maleate inhibitors, fumarate inhibitors, organophosphorus inhibitors and acetylene inhibitors.

[0013] Preferably, the mass fraction of the Castel catalyst is 0.2wt% to 1wt%.

[0014] The preparation method of the organic silicon thermal conductive adhesive comprises mixing the components evenly according to a proportion, and then performing a vacuum degassing treatment.

[0015] Preferably, in the preparation method, a planetary mixer is used for mixing.

[0016] More preferably, in the preparation method, the planetary mixer parameters are set as follows: stirring speed of 200 to 8000 r / min, stirring time of 30 to 120 min, dispersion speed of 1500 to 3500 r / min, dispersion time of 60 to 160 min, vacuum degassing pressure of -0.08 to -0.1 MPa, and time of 5 to 20 min.

[0017] By adopting the above technical solution, part of the alumina powder is attached to the alumina fiber, and after the adhesive is thermally cured and formed, a heat-conducting network structure is formed, which further increases the density of the heat-conducting path and improves the thermal conductivity of the silicone thermal conductive adhesive. At the same time, the alumina fiber is also used as a reinforcing material. After the adhesive is thermally cured and formed, an interface structure of you in me and me in you is formed between the polymer matrix and the fiber, which improves the mechanical properties of the silicone adhesive.

[0018] A test method for the above-mentioned organic silicone adhesive is to first pour the prepared adhesive into a mold, heat it to 120-160°C for 1-3 hours, and solidify it into a shape. The thermal conductivity is mainly evaluated by the thermal conductivity, and the test is performed using a thermal conductivity meter. The mechanical properties are mainly evaluated by the tensile strength, and the test is performed using a universal tensile testing machine.

[0019] The beneficial effects of the present invention are:

[0020] The organic silicone adhesive of the present invention benefits from the synergistic effect of the fibers and the powder, which jointly build a heat-conducting network pathway structure, thereby improving the thermal conductivity of the organic silicone adhesive, and the powder adheres to the fibers and is not prone to separation, sedimentation, and compaction.

[0021] In the organic silicone adhesive of the present invention, when the polymer matrix is ​​subjected to force, the deformation will be transmitted to the fiber, the fiber deformation is small, and the matrix deformation is large, most of the force will be transmitted to the fiber, becoming the main force point, thereby improving the mechanical properties of the organic silicone adhesive. DETAILED DESCRIPTION

[0022] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0023] In the following examples: tensile strength, MPa, national standard test method GB / T 528-2009; elongation at break, %, national standard test method GB / T 528-2009; thermal conductivity W / m·K, international standard test method ISO 22007-2)

[0024] The sources of raw materials used in the present invention are shown in the following table:

[0025] Chemical reagent name Manufacturer Vinyl silicone oil Shandong Dayi Chemical Co., Ltd. Methyl MQ silicone resin Shanghai Yuanye Biotechnology Co., Ltd. Hydrogen silicone oil Tianjin Xiensi Biochemical Technology Co., Ltd. Alumina Fiber Shandong Luyang Energy Saving Materials Co., Ltd. Alumina powder Shanghai Aladdin Biochemical Technology Co., Ltd. Inhibitors Beijing Bailingwei Technology Co., Ltd. Custer Catalyst Beijing Inotech Technology Co., Ltd.

[0026] Example 1

[0027] A silicone thermally conductive adhesive comprises components, measured by weight, including 100 parts of vinyl silicone oil, 20 parts of methyl MQ silicone resin, 10 parts of hydrogen-containing silicone oil, 60 parts of thermally conductive filler, 0.5 parts of inhibitor and 0.8 parts of Custer catalyst, wherein the viscosity of the vinyl silicone oil is about 2500 mPa·s, the hydrogen content of the hydrogen-containing silicone oil is 1.20wt%, the thermally conductive filler comprises alumina fiber and alumina powder, the mass ratio of the two is fiber:powder=1:3, the diameter of the alumina fiber is about 5μm, the length is about 10μm, and the average particle size of the alumina powder is 5μm.

[0028] The above components were stirred and dispersed by a planetary mixer and then subjected to vacuum degassing treatment. The stirring speed was 200 r / min, the stirring time was 30 min, the dispersion speed was 1500 r / min, the dispersion time was 60 min, and the vacuum degassing pressure was -0.05 MPa for 5 min.

[0029] The curing temperature of the obtained organic silicone thermal conductive adhesive was 150° C., the curing time was 2 h, and the thermal conductivity after curing was 3.67 W / m·K. The tensile strength was 1.59 MPa, and the elongation at break was 100%.

[0030] Example 2

[0031] A silicone thermally conductive adhesive comprises components, measured by weight, including 100 parts of vinyl silicone oil, 20 parts of methyl MQ silicone resin, 10 parts of hydrogen-containing silicone oil, 60 parts of thermally conductive filler, 0.5 parts of inhibitor and 0.8 parts of Custer catalyst, wherein the viscosity of the vinyl silicone oil is 2500 mPa·s, the hydrogen content of the hydrogen-containing silicone oil is 1.20wt%, and the thermally conductive filler comprises alumina fiber and alumina powder, the mass ratio of the two is fiber:powder=1:5, the diameter of the alumina fiber is about 7μm, the length is about 30μm, and the average particle size of the alumina powder is 7μm.

[0032] The mixture was stirred and dispersed evenly by a planetary mixer, and then vacuum degassing was performed. The stirring speed was 400 r / min, the stirring time was 60 min, the dispersion speed was 2000 r / min, the dispersion time was 90 min, and the vacuum degassing pressure was -0.1 MPa for 5 min.

[0033] The curing temperature of the obtained organic silicon thermal conductive adhesive was 150° C. and the curing time was 2 h. After curing, the thermal conductivity was measured to be 4.83 W / m·K. The tensile strength was 1.98 MPa and the elongation at break was 120%.

[0034] Example 3

[0035] A silicone thermally conductive adhesive comprises components, measured by weight, of 100 parts of vinyl silicone oil, 20 parts of methyl MQ silicone resin, 10 parts of hydrogen-containing silicone oil, 60 parts of thermally conductive filler, 0.5 parts of inhibitor and 0.8 parts of Custer catalyst, wherein the viscosity of the vinyl silicone oil is 2500 mPa·s, the hydrogen content of the hydrogen-containing silicone oil is 1.20wt%, and the thermally conductive filler comprises alumina fiber and alumina powder, the mass ratio of the two is fiber:powder=1:7, the diameter of the alumina fiber is about 10 μm, the length is about 50 μm, and the average particle size of the alumina powder is about 10 μm.

[0036] The above components were stirred and dispersed by a planetary mixer and then subjected to vacuum degassing treatment. The stirring speed was 600 r / min, the stirring time was 90 min, the dispersion speed was 3000 r / min, the dispersion time was 120 min, and the vacuum degassing pressure was -0.1 MPa for 10 min.

[0037] The curing temperature of the obtained organic silicone thermal conductive adhesive was 150° C., the curing time was 2 h, and the thermal conductivity after curing was measured to be 5.76 W / m·K. The tensile strength was 2.27 MPa, and the elongation at break was 139%.

[0038] Comparative Example 1

[0039] Comparative Example 1 is based on Example 2, and differs from Example 2 in that the thermally conductive filler is alumina powder.

[0040] After curing and molding, the thermal conductivity of Comparative Example 2 was measured to be 1.87 W / m·K, the tensile strength was 0.97 MPa, and the elongation at break was 100%.

[0041] Comparative Example 2

[0042] Comparative Example 2 is based on Example 2, and differs from Example 2 in that the average particle size of the alumina powder is 3 μm.

[0043] After curing and molding, the thermal conductivity of Comparative Example 2 was measured to be 2.86 W / m·K, the tensile strength was 1.08 MPa, and the elongation at break was 97%.

[0044] Comparative Example 3

[0045] Comparative Example 3 is based on Example 2, and differs from Example 2 in that the length of the alumina fiber is 60 μm.

[0046] After curing and molding, the thermal conductivity of comparative example 3 was measured to be 2.76 W / m·K, the tensile strength was 1.32 MPa, and the elongation at break was 90%.

[0047] Comparative Example 4

[0048] Comparative Example 4 is based on Example 2, and differs from Example 2 in that the thermal conductive filler is alumina fiber.

[0049] After curing and molding, the thermal conductivity of Comparative Example 4 was measured to be 1.59 W / m·K, the tensile strength was 0.89 MPa, and the elongation at break was 100%.

[0050] By comparing Examples 1 to 3 with Comparative Examples 1 to 4, it can be seen that the doping of alumina fibers and alumina powders and the matching of the fiber aspect ratio and the powder particle size in the present invention, especially when the alumina fiber diameter is consistent with the powder particle size, can further improve the thermal conductivity and mechanical properties of the silicone adhesive.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Those skilled in the art should understand that the technical solution of the present invention can be deduced or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A silicone thermally conductive adhesive, characterized in that: Its components, measured by weight, include: 90-150 parts of vinyl silicone oil, 10-70 parts of methyl MQ silicone resin, 5-30 parts of hydrogen-containing silicone oil, 50-80 parts of thermal conductive filler, 0.1-1 part of inhibitor, and 0.1-2 parts of Custer catalyst; wherein the thermal conductive filler is alumina fiber and alumina powder.

2. The organic silicone thermally conductive adhesive according to claim 1, characterized in that: The mass ratio of the alumina fiber to the alumina powder is 1:3 to 1:

9.

3. The organic silicone thermally conductive adhesive according to claim 1, characterized in that: The vinyl silicone oil is a branched-chain vinyl silicone oil, a linear-chain vinyl silicone oil, or a mixture of one or more linear and branched-chain vinyl silicone oils.

4. The organic silicone thermally conductive adhesive according to claim 3, characterized in that: The viscosity of the vinyl silicone oil is in the range of 1000 to 5000 mPa·s.

5. The organic silicone thermally conductive adhesive according to claim 1, characterized in that: The particle size of the methyl MQ silicone resin is in the range of 50 to 150 μm.

6. The organic silicone thermally conductive adhesive according to claim 1, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 1 wt% to 1.45 wt%.

7. The organic silicone thermally conductive adhesive according to claim 1, characterized in that: The diameter of the alumina fiber is 5 to 10 μm, and the length is 10 to 50 μm; the average particle size of the alumina powder is 5 to 10 μm.

8. The organic silicone thermally conductive adhesive according to claim 1, characterized in that: The inhibitor is selected from one or two of maleate inhibitors, fumarate inhibitors, organophosphorus inhibitors and acetylene inhibitors; the mass fraction of the Custer catalyst is 0.2wt% to 1wt%.

9. The method for preparing the organic silicone thermally conductive adhesive according to any one of claims 1 to 8, characterized in that: Mix all components evenly according to the proportion, and then carry out vacuum degassing treatment.

10. The method for preparing the organic silicone thermal conductive adhesive according to claim 9, characterized in that: In the preparation method, a planetary mixer is used for mixing, and the parameters of the planetary mixer are set as follows: a stirring speed of 200 to 8000 r / min, a stirring time of 30 to 120 min, a dispersion speed of 1500 to 3500 r / min, a dispersion time of 60 to 160 min, a vacuum degassing pressure of -0.08 to -0.1 MPa, and a time of 5 to 20 min.