Tungsten / titanium nitride etching solution capable of avoiding intermetallic electrochemical corrosion effect
By using etching liquid composed of hydrogen peroxide, inorganic alkali, metal ion masking agent and electrochemical corrosion inhibitor in IGBT chip manufacturing, the electrochemical corrosion problem between the tungsten and titanium nitride layers is solved, and a stable etching rate is achieved and lifespan ensures chip quality.
Patent Information
- Application Number
- CN202410839568.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-06-26
AI Technical Summary
During the manufacturing process of IGBT chips, electrochemical corrosion is prone to occur between metal layers such as tungsten and titanium nitride, resulting in uneven etching speed and uneven side etching, affecting the quality of the chip.
Using an etching solution composed of hydrogen peroxide, inorganic alkali, metal ion masking agent, electrochemical corrosion inhibitor and surfactant, the tungsten layer and titanium/ Electrochemical corrosion between titanium nitride layers.
It effectively avoids the electrochemical corrosion effect between metals, maintains a stable etching rate and life, ensures uniform etching of each layer of metal, reduces metal tailing phenomenon, and improves the process reliability of the chip.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal wet etching and IGBT chip crossover, and in particular relates to a tungsten / titanium nitride etching solution for avoiding electrochemical corrosion effects between metals and a use method thereof. Background Art
[0002] In the manufacturing of automotive chips, IGBT chips are usually used in scenarios involving voltage conversion, and the contacts or interconnects in the IGBT are usually made of tungsten, titanium, copper and other metals and their alloys to form a stacked structure. This structure is very prone to electrochemical corrosion due to the galvanic effect. The greater the difference in activity between the metals, the more serious the electrochemical corrosion effect. Therefore, in the etching process of each layer of metal, it is easy for different metals to have different etching speeds, and the side etching and etching cone angles of each layer of metal are uneven. In the etching of tungsten / titanium nitride metal stacks, metal tungsten loses electrons as an anode, and the metal titanium / titanium nitride layer gains electrons. The electrochemical corrosion of the tungsten layer and its inherently active chemical activity make the etching rate of tungsten much higher than that of the titanium / titanium nitride layer. Therefore, it is particularly important to develop a tungsten / titanium nitride etching solution that can avoid the electrochemical corrosion effect between metals. Summary of the invention
[0003] The object of the present invention is to provide a tungsten / titanium nitride etching solution and a method for using the same for avoiding electrochemical corrosion between metals.
[0004] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions: A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion effects between metals, the etching solution comprising the following components by mass percentage: 10%-30% hydrogen peroxide, 1%-5% alkali, 1%-5% surfactant, 0.1%-2% electrochemical corrosion inhibitor, and the balance being deionized water.
[0005] Preferably, the etching solution further comprises the following components by mass percentage: 0.1%-1% of a metal ion masking agent.
[0006] Preferably, the base is potassium hydroxide, ammonia water or tetramethylammonium hydroxide or a combination thereof.
[0007] Preferably, the surfactant is acetamide, isobutylamide, chloroacetamide or N-vinylacetamide or a combination thereof.
[0008] Preferably, the electrochemical corrosion inhibitor is dodecylphosphonic acid, phenylphosphinic acid, 1,4-butanediphosphonic acid or 4-aminobutylphosphonic acid or a combination thereof.
[0009] Further preferably, the metal ion masking agent is cyclobenzaprine hydrochloride, chlormezaprine, bezafibrate or cyclobenzaprine or a combination thereof. Compared with the prior art, the present invention has the following beneficial effects: The advantages and beneficial effects of the present invention are as follows: the etching solution is composed of hydrogen peroxide, inorganic alkali, metal ion masking agent, electrochemical corrosion inhibitor, surfactant and deionized water. The alkali is at least one of potassium hydroxide, ammonia water and tetramethylammonium hydroxide, and the alkali is used to adjust the pH value of the etching solution to stabilize the etching rate; hydrogen peroxide is an oxidant; the metal ion masking agent can complex with metal tungsten ions, inhibit the oxidation of tungsten, reduce the etching speed of the etching solution on metal tungsten, and improve the etching selectivity. The electrochemical corrosion inhibitor can significantly reduce the electrochemical corrosion reaction potential between the tungsten layer and the titanium / titanium nitride layer, inhibit the corrosion current between the tungsten layer and the titanium / titanium nitride layer, and weaken the electrochemical corrosion between the two metal layers. At the same time, the surfactant can adjust the wetting and contact between the etching solution and different film layers. Ensure that each film layer is completely etched to avoid the occurrence of metal tailing and other phenomena that affect the subsequent process. The tungsten / titanium nitride etching solution capable of avoiding electrochemical corrosion between metals in the present invention can significantly reduce the electrochemical corrosion between the metal tungsten layer and the titanium / titanium nitride layer compared with ordinary etching solutions, while also maintaining a stable etching rate and life. DETAILED DESCRIPTION
[0010] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0011] The etching temperature and etching time were 60°C and 5 min, respectively.
[0012] Prepare the etching solution in a beaker according to its composition, weigh 50g of the etching solution after ultrasonic stirring and put it into a constant temperature water bath at 60℃, and after the etching solution temperature reaches 60℃ and stabilizes for a period of time, cut the tungsten and titanium nitride single-layer metal membranes into 1.6cm×1.6cm sizes with a knife, rinse with ultrapure water, and blow clean with nitrogen; use a four-probe thickness gauge to measure the film thickness of the tungsten and titanium nitride sheets before etching, then fix the tungsten and titanium nitride sheets back to back (silicon base layers are bonded), and connect the working electrodes of the electrochemical workstation to the tungsten and titanium nitride metal layers respectively, so as to measure the corrosion current Icorr flowing between tungsten and titanium nitride during the etching process. During etching, the test piece is fixed with a clamp, suspended and immersed in a continuously circulating etching solution at 60°C. After etching for 5 minutes, the tungsten and titanium nitride sheets are taken out, rinsed with ultrapure water, purged with nitrogen, and the film thickness of tungsten and titanium nitride after etching is tested with a four-probe thickness gauge. The corrosion rate of the metal by the etching solution is obtained by the difference in film thickness before and after etching. The corrosion current Icorr measured by the constant potentiostat of the electrochemical workstation is used to characterize the intensity of the electrochemical corrosion occurring during this etching.
[0013] Example 1 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% potassium hydroxide, and the balance ultrapure water.
[0014] Example 2 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, and the balance ultrapure water.
[0015] Example 3 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% tetramethylammonium hydroxide, and the balance ultrapure water.
[0016] Example 4 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% acetamide, and the balance ultrapure water.
[0017] Example 5 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutylamide, and the balance ultrapure water.
[0018] Example 6 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% chloroacetamide, and the balance ultrapure water.
[0019] Example 7 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% N-vinyl acetamide, and the balance ultrapure water.
[0020] Example 8 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine hydrochloride, and the balance ultrapure water.
[0021] Example 9 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% chloromezazone, and the balance ultrapure water.
[0022] Example 10 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% bezafibrate, and the balance ultrapure water.
[0023] Embodiment 11 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine, and the balance ultrapure water.
[0024] Example 12 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutylamide, 0.5wt% dodecylphosphonic acid, and the balance ultrapure water.
[0025] Example 13 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutylamide, 0.5wt% phenylphosphinic acid, and the balance ultrapure water.
[0026] Embodiment 14 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0027] Embodiment 15 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% 4-aminobutylphosphonic acid, and the balance ultrapure water.
[0028] Example 16 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine hydrochloride, 0.5wt% dodecylphosphonic acid, and the balance ultrapure water.
[0029] Embodiment 17 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine hydrochloride, 0.5wt% phenylphosphinic acid, and the balance ultrapure water.
[0030] Embodiment 18 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine hydrochloride, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0031] Embodiment 19 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine hydrochloride, 0.5wt% 4-aminobutylphosphonic acid, and the balance ultrapure water.
[0032] Embodiment 20 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% chloromezazone, 0.5wt% dodecylphosphonic acid, and the balance ultrapure water.
[0033] Embodiment 21 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% chloromezazone, 0.5wt% phenylphosphinic acid, and the balance ultrapure water.
[0034] Embodiment 22 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% chloromezazone, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0035] Embodiment 23 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% chloromezazone, 0.5wt% 4-aminobutylphosphonic acid, and the balance ultrapure water.
[0036] Embodiment 24 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% bezafibrate, 0.5wt% dodecylphosphonic acid, and the balance ultrapure water.
[0037] Embodiment 25 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% bezafibrate, 0.5wt% phenylphosphinic acid, and the balance ultrapure water.
[0038] Embodiment 26 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% bezafibrate, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0039] Embodiment 27 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% bezafibrate, 0.5wt% 4-aminobutylphosphonic acid, and the balance ultrapure water.
[0040] Embodiment 28 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine, 0.5wt% dodecylphosphonic acid, and the balance ultrapure water.
[0041] Embodiment 29 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine, 0.5wt% phenylphosphinic acid, and the balance ultrapure water.
[0042] Embodiment 30 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0043] Embodiment 31 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 1wt% isobutyramide, 0.5wt% cyclobenzaprine, 0.5wt% 4-aminobutylphosphonic acid, and the balance ultrapure water.
[0044] Comparative Example 1 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% cyclobenzaprine hydrochloride, and the balance ultrapure water.
[0045] Comparative Example 2 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% chloromethadone, and the balance ultrapure water.
[0046] Comparative Example 3 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% bezafibrate, and the balance ultrapure water.
[0047] Comparative Example 4 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% cyclobenzaprine, and the balance ultrapure water.
[0048] Comparative Example 5 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% dodecylphosphonic acid, and the balance ultrapure water.
[0049] Comparative Example 6 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% phenylphosphinic acid, and the balance ultrapure water.
[0050] Comparative Example 7 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0051] Comparative Example 8 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% 4-aminobutylphosphonic acid, and the balance ultrapure water.
[0052] Comparative Example 9 A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, comprising: 20wt% hydrogen peroxide, 5wt% ammonia water, 0.5wt% chloromezazone, 0.5wt% 1,4-butanediphosphonic acid, and the balance ultrapure water.
[0053] Detection method: The etching time of tungsten (Å / min) is fixed, and the film thickness of the tungsten sheet before and after etching is measured using a four-probe thickness gauge to obtain the etching rate of tungsten. The etching time of titanium nitride (Å / min) is fixed, and the film thickness of the titanium nitride sheet before and after etching is measured using a four-probe thickness gauge to obtain the etching rate of titanium nitride.
[0054] Corrosion current Icorr (A): During the etching process, the corrosion current Icorr flowing between tungsten and titanium nitride is directly measured using the working electrode of the electrochemical workstation.
[0055] The experimental results are shown in Table 1: In Examples 1-3, because no ingredients other than oxidants, alkalis, and ultrapure water were added, the etching rates of the three formulations for tungsten were all above 300Å / min, and more metal residues were left. At the same time, the corrosion currents measured by the electrochemical workstation were all greater than 3×10 -6 A.
[0056] In Examples 4-7, the addition of surfactant improves the metal residue problem during the etching process, wherein Examples 5 and 6 both have trace metal residues, but the addition of surfactant also slightly increases the etching rate of tungsten.
[0057] In Examples 8-15, a single component metal ion masking agent or electrochemical corrosion inhibitor was added to the formula based on hydrogen peroxide, alkali, and surfactant. In Examples 8-11, the addition of different types of metal ion masking agents showed different complexing abilities with tungsten ions, which reduced the etching rate of tungsten to a certain extent, all below 300Å / min. However, since the corrosion current was still not suppressed at this time, the overall inhibitory effect of the etching solution on tungsten was still insufficient. In Examples 12-15, the addition of different electrochemical corrosion inhibitors, only Example 14 significantly reduced the corrosion current, making Icurr below 1×10 -6 A, which shows that the presence of electrochemical corrosion inhibitor plays a key role in inhibiting the etching of tungsten.
[0058] In Examples 16-31, the metal ion masking agent and the electrochemical corrosion inhibitor used in Examples 8-15 were cross-combined, and the effect of Example 22 was the most significant. Under the combined effect of the metal ion masking agent and the electrochemical corrosion inhibitor, the etching rate of tungsten was 2.7Å / min, and the corrosion current was 0.2×10 -7 A, the selectivity of tungsten / titanium nitride reaches 1:5.74. This shows that when the metal ion masking agent and the electrochemical corrosion inhibitor are both present in the formula, the complexation effect of the formula components on tungsten and the inhibition of corrosion current are the same, the etching rate of the etching solution on tungsten can be further reduced, and the selectivity of tungsten / titanium nitride is further improved. When the metal ion masking agent and the electrochemical corrosion inhibitor in the etching solution formula are both preferred components, the etching solution can have the characteristics of avoiding the electrochemical corrosion effect between metals. Table 1
[0059] The technical solution of the present invention is explained through the above embodiments, but the present invention is not limited to the above embodiments, that is, it does not mean that the present invention must rely on the above specific embodiments to be implemented. Any improvements made by technicians in the relevant field based on the present invention, or equivalent replacement of the materials selected by the present invention, etc., fall within the scope of protection of the patent.
Claims
1. A tungsten / titanium nitride etching solution for avoiding electrochemical corrosion between metals, characterized in that: The etching solution comprises the following components by mass percentage: 10% to 30% hydrogen peroxide, 1% to 5% alkali, 1% to 5% surfactant, 0.1% to 2% electrochemical corrosion inhibitor, and the balance is deionized water.
2. The tungsten / titanium nitride etching solution for avoiding intermetallic electrochemical corrosion effect according to claim 1, characterized in that: The etching solution also includes the following components in percentage by mass: 0.1% to 1% of a metal ion masking agent.
3. The tungsten / titanium nitride etching solution for avoiding intermetallic electrochemical corrosion effect according to claim 1, characterized in that: The alkali is potassium hydroxide, ammonia water or tetramethylammonium hydroxide or a combination thereof.
4. The tungsten / titanium nitride etching solution for avoiding intermetallic electrochemical corrosion effect according to claim 1, characterized in that: The surfactant is acetamide, isobutylamide, chloroacetamide or N-vinyl acetamide or a combination thereof.
5. The tungsten / titanium nitride etching solution for avoiding intermetallic electrochemical corrosion effect according to claim 1, characterized in that: The electrochemical corrosion inhibitor is dodecylphosphonic acid, phenylphosphinic acid, 1,4-butanediphosphonic acid or 4-aminobutylphosphonic acid or a combination thereof.
6. The tungsten / titanium nitride etching solution for avoiding intermetallic electrochemical corrosion effect according to claim 2, characterized in that: The metal ion masking agent is cyclobenzaprine hydrochloride, chlormezaprine, bezafibrate or cyclobenzaprine or a combination thereof.
Citation Information
Patent Citations
Compositions and methods for selectively etching titanium nitride
CN105683336A
Etching composition for mono-layed film or multi-layed film and etching method using the same
CN107304476A
Composition for selectively removing titanium nitride hard mask and / or etching residues
CN110095952A
Compositions and methods for selectively etching titanium nitride
CN111394100A
Hydrogen peroxide decomposition inhibitor
CN113939899A