Arsenic-polluted soil remediation material and preparation method thereof

Through iron-modified bamboo carbon, humic acid and iron-modified pyrolytic manganese slag combination materials, the precipitation of iron-manganese nodules and humic acid is used to solve the problem of arsenic pollution in the soil, and the solidification of arsenic and soil ecosystem are achieved. Improved stability.

CN118931547APending Publication Date: 2024-11-12LANZHOU RESOURCES & ENVIRONMENT VOC TECH COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981088.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12
Patent Text Reader

Abstract

The invention belongs to the technical field of soil remediation application, and particularly relates to an arsenic-polluted soil remediation material and a preparation method thereof. Comprising the following components: 50-70 parts of iron modified bamboo charcoal; 10 to 20 parts of humic acid; and 20 to 30 parts of iron modified pyrolysis manganese slag. According to the arsenic-contaminated soil remediation material and the preparation method thereof, oxidation of ferrous ions can be promoted through Mn, arsenic can be solidified through secondary iron minerals formed by ferric ion oxide generated by oxidation of the ferrous ions, meanwhile, Mn serves as a strong oxidant and can form iron manganese nodules through migration and aggregation, and therefore the arsenic-contaminated soil remediation material is obtained. According to the present invention, with the application of the bamboo charcoal, the trivalent arsenic ions are oxidized into the pentavalent arsenic ions so as to reduce the toxicity, and the humic acid and the iron ions can further form the precipitate by using the alkaline characteristic of the bamboo charcoal so as to achieve the purposes of As curing and stabilization, As migration reduction and As bioavailability reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of soil remediation applications, and in particular relates to an arsenic-contaminated soil remediation material and a preparation method thereof. Background Art

[0002] In recent decades, heavy metal pollution of agricultural ecosystems has become a hot topic in environmental research. In addition to natural pollution sources such as soil parent materials, heavy metals in soil are also related to human activities, such as the abuse of herbicides, pesticides and fertilizers, sewage irrigation, etc. The toxicity, persistence and bioaccumulation of heavy metal elements will significantly interfere with the normal functions of ecosystems, leading to a decline in soil quality and fertility, which not only undermines food security, but also poses a threat to human health. Among these heavy metal elements, arsenic (As), as a highly toxic metalloid element, poses a much higher health risk than elements such as cadmium (Cd) and chromium (Cr).

[0003] Arsenic (As) is a metalloid substance that exists in the form of a silver-grey crystalline solid. It is usually associated with metal elements such as Au, Cu, Pb, Zn, Ni and Co in the form of sulfides in mining areas. Arsenic in the environment mainly exists in the form of elemental arsenic, inorganic arsenic and organic arsenic. Among them, inorganic arsenic mainly exists in the form of trivalent and invalent oxygen-containing salts. The oxidized form of arsenate has a strong affinity with other elements and has a low solubility. The reduced form of arsenite is more soluble, so arsenic is more mobile under reducing conditions. The biological toxicity of As in different forms and valence states varies greatly. As(III) is more toxic than organic arsenic and As(V). Arsenic can be used to make paints, wood preservatives, metal alloys for electronic circuits and pesticides. It also has important medicinal value in the treatment of lymphoma and leukemia. For example, arsenic trioxide is the first choice for the treatment of acute promyelocytic leukemia. While it is widely used in medicine, industry and agriculture, arsenic pollution also poses a serious threat to human health. Arsenic has been identified as an environmental toxin and carcinogen by different institutions. Arsenic in the environment enters the human body mainly through ingestion, inhalation and skin absorption. Both trivalent and pentavalent arsenic compounds can be quickly absorbed by the stomach and intestines. Arsenic accumulation is most prominent in the liver, kidneys and muscles. Only about 70% of the arsenic (inorganic arsenic and organic arsenic) that enters the human body can be excreted through the kidney system through urine. Once arsenic enters the human body, it will cause a wide range of acute and chronic toxic effects. Keratosis or skin disease is one of the most common symptoms of chronic arsenic exposure in the early stage. As a carcinogen, long-term exposure to arsenic can lead to the occurrence of liver cancer, lung cancer, bladder cancer and other cancers.

[0004] Heavy metal pollution in soil is hidden, non-degradable and cumulative, which will directly endanger the safety of agricultural products. Crops can absorb heavy metals in the soil through their roots, transport them to the aboveground parts, and accumulate them in the edible parts, which can threaten human health through the "soil-human body" and "soil-crop-human body". Therefore, how to repair the soil and reduce or solidify the heavy metal pollution in the soil is a problem that needs to be solved at present. Summary of the invention

[0005] In view of the technical problems existing in the above-mentioned arsenic pollution in soil, the present invention proposes an arsenic-contaminated soil remediation material and a preparation method thereof which has a simple method and operation method and can effectively reduce arsenic pollution in soil.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is that the present invention provides an arsenic contaminated soil remediation material, comprising the following components:

[0007] 50-70 parts of iron-modified bamboo charcoal;

[0008] Humic acid 10 to 20 parts;

[0009] 20 to 30 parts of iron-modified pyrolytic manganese slag.

[0010] The present invention also provides a method for preparing the above-mentioned arsenic-contaminated soil remediation material, which is characterized by comprising the following steps:

[0011] a. First, the alpine bamboo is dried at 80°C, and then the dried alpine bamboo is added into a quartz crucible and placed into a tubular furnace. After nitrogen is introduced, it is heated to 1000°C for 30 minutes to obtain bamboo charcoal for standby use;

[0012] b. Then, the bamboo charcoal is crushed and passed through a 100-mesh sieve to obtain bamboo charcoal particles. Then, the bamboo charcoal particles are added to a potassium hydroxide solution and stirred evenly to activate the solution.

[0013] c. Then, continue to add ferric nitrate to the potassium hydroxide solution and continue stirring until a red precipitate is produced;

[0014] d. Then, dilute with water, transfer to an oven and keep at 70°C for 60 hours, then stand at room temperature for 12 hours, wash, filter, dry, and dry to constant weight to obtain iron-modified bamboo charcoal for later use;

[0015] e. Then, the manganese slag was ground and passed through a 100-mesh sieve. After drying, it was added to the FeCl3 solution and mixed. The mixture was stirred for 2 h using a magnetic stirrer. After standing for 12 h, the mixture was filtered and rinsed with deionized water until the filtrate was clear. The mixture was then dried in an oven at 105°C for later use.

[0016] f. Then, the dried manganese slag is added into a quartz crucible and placed into a tubular furnace. After nitrogen is introduced, the mixture is heated to 500° C. for 30 min to obtain iron-modified pyrolytic manganese slag for standby use.

[0017] g. Finally, add ultrapure water to moisten the humic acid, iron-modified bamboo charcoal, and iron-modified pyrolytic manganese slag, mix them thoroughly, and dry them at 80°C to constant weight. The desired arsenic-contaminated soil remediation material can be obtained.

[0018] Preferably, in step c, the mass ratio of bamboo charcoal particles to ferric nitrate is 1:1.

[0019] Compared with the prior art, the advantages and positive effects of the present invention are:

[0020] The invention provides an arsenic-contaminated soil restoration material and a preparation method thereof. Mn can be used to promote the oxidation of divalent iron ions, and secondary iron minerals formed by trivalent iron ion oxides generated by the oxidation of divalent iron ions can solidify arsenic. At the same time, Mn, as a strong oxidant, can migrate and aggregate to form iron-manganese nodules, oxidizing trivalent arsenic ions into pentavalent arsenic ions, thereby reducing toxicity. At the same time, the alkaline property of bamboo carbon itself is utilized to enable humic acid to further form precipitation with iron ions, thereby achieving the purpose of solidifying and stabilizing As and reducing its migration and bioavailability. DETAILED DESCRIPTION

[0021] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described below in conjunction with embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0022] In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention may also be implemented in other ways than those described herein. Therefore, the present invention is not limited to the specific embodiments of the following disclosure.

[0023] Example 1: This example provides an arsenic contaminated soil remediation material and a preparation method thereof

[0024] In this embodiment, there are three main components, namely 50 parts of iron-modified bamboo charcoal, 20 parts of humic acid and 30 parts of iron-modified pyrolytic manganese slag.

[0025] Among the above materials, biochar can not only be used as an amendment to improve soil structure and properties, but also has the potential to passivate heavy metals through complexation, chelation, precipitation, adsorption, pore filling and other effects due to its rich oxygen-containing functional groups, huge specific surface area and developed pore structure. In this embodiment, bamboo charcoal is used for two purposes. One is to utilize the larger specific surface area of ​​bamboo charcoal, which is between 189.6 and 517.28 m2 / g, has a strong adsorption capacity, can effectively adsorb heavy metals, and another point is to use the alkalinity of bamboo charcoal. The pH of traditional straw biochar is generally weakly alkaline, while the pH value of bamboo charcoal is between 9.8 and 10.05. Humic acid can form precipitation with iron ions under alkaline conditions, and the precipitation process will solidify arsenic ions, thereby preventing their migration. Iron-modified bamboo charcoal has higher hydrophilicity and polarity than unmodified bamboo charcoal. Fe-O groups are formed. As a result, complexation and co-precipitation reactions occur with arsenic ions, reducing their migration and bioavailability.

[0026] At the same time, it can change the form of heavy metals in the soil, reduce the biological effectiveness of heavy metals, and thus reduce their toxic effects on crops; humic acid can reduce the activity of organic pollutants in the soil, making them lose their harm to the soil and crops; humic acid can promote the activity and reproduction of microorganisms in the soil, increase the number and activity of microorganisms in the soil, improve the biological fertility of the soil, and is beneficial to the balance and stability of the soil ecosystem.

[0027] In addition, arsenic in soil is mainly present as AsO4 3- The form of Fe 2+ , Fe 3+ Both can be used with AsO4 3- Mn can promote the oxidation of divalent iron ions, and the secondary iron minerals formed by the trivalent iron ion oxides produced by the oxidation of divalent iron ions can solidify arsenic. At the same time, Mn, as a strong oxidant, can form iron-manganese nodules through migration and aggregation, oxidizing trivalent arsenic ions into pentavalent arsenic ions, thereby reducing toxicity.

[0028] To this end, using the above mechanism, the preparation method of the arsenic contaminated soil remediation material provided in this embodiment is as follows: first, the alpine bamboo is dried at 80°C, and then the dried alpine bamboo is added to a quartz crucible and placed in a tubular furnace, and after nitrogen is introduced, it is heated to 1000°C and kept warm for 30 minutes to obtain bamboo charcoal for later use;

[0029] Then, the bamboo charcoal is crushed and passed through a 100-mesh sieve to obtain bamboo charcoal particles. Then, the bamboo charcoal particles are added to a potassium hydroxide solution and stirred evenly to activate it; then, ferric nitrate is continued to be added to the potassium hydroxide solution and stirred continuously until a red precipitate is produced, and the mass ratio of bamboo charcoal particles to ferric nitrate is 1:1; then, water is added to dilute it, and then, it is transferred to an oven and kept at 70°C for 60 hours, and then, it is allowed to stand at room temperature for 12 hours, washed, filtered, dried, and dried to constant weight to obtain iron-modified bamboo charcoal for use; then, the manganese slag is ground and passed through a 100-mesh sieve. After drying, it is added to the FeCl3 solution and mixed, stirred for 2 hours with a magnetic stirrer, allowed to stand for 12 hours, filtered, and rinsed with deionized water until the filtrate is clear, and then dried in an oven at 105°C for use.

[0030] Then, the dried manganese slag is added into a quartz crucible and placed into a tubular furnace. After nitrogen is introduced, it is heated to 500° C. and kept warm for 30 minutes to obtain iron-modified pyrolytic manganese slag for later use.

[0031] Finally, humic acid, iron-modified bamboo charcoal, and iron-modified pyrolytic manganese slag are moistened with ultrapure water and fully mixed, and then dried at 80° C. to a constant weight, thereby obtaining the desired arsenic-contaminated soil remediation material.

[0032] Experiment: 0-20cm of arsenic-contaminated surface soil was dug, and impurities such as stones, animal and plant remains in the soil were removed. The soil samples were then naturally air-dried, ground through a 100-mesh sieve, and put into a sealed bag. The effective arsenic content was measured to be 0.268mg / kg.

[0033] Take 100g of the above soil and add it to a culture bottle. Apply the arsenic-contaminated soil remediation material prepared in Example 1 to the soil at a ratio of 2% (w / w). Place it in a fully automatic turning machine and turn it for 24 hours to mix the material and soil evenly. Add an appropriate amount of deionized water (60% of the field water holding capacity) to the culture bottle, stir it thoroughly and place it for cultivation. During the cultivation process, the constant weight method is used to replenish water in time so that the soil moisture content is consistent with the initial cultivation. Three replicates are set for each treatment. Samples are taken 30 days after cultivation, and the effective arsenic content is determined to be 0.205 mg / kg.

[0034] The experimental results show that applying arsenic-contaminated soil remediation materials to the soil has a certain stabilizing effect on soil As, and the content of available As in the soil is reduced by 23.5%.

[0035] Example 2: This example provides an arsenic contaminated soil remediation material and a preparation method thereof

[0036] In this embodiment, there are three main components, namely 70 parts of iron-modified bamboo charcoal, 10 parts of humic acid and 20 parts of iron-modified pyrolytic manganese slag.

[0037] The same preparation method and experimental means as in Example 1 were used. The experimental results showed that applying the arsenic-contaminated soil remediation material to the soil had a certain stabilizing effect on soil As, the effective As content in the soil was 0.201 mg / kg, and the effective As content in the soil was reduced by 23.5%.

[0038] Example 3: This example provides an arsenic contaminated soil remediation material and a preparation method thereof

[0039] In this embodiment, there are three main components, namely 60 parts of iron-modified bamboo charcoal, 15 parts of humic acid and 25 parts of iron-modified pyrolytic manganese slag.

[0040] The same preparation method and experimental means as in Example 1 were used. The experimental results showed that applying the arsenic-contaminated soil remediation material to the soil had a certain stabilizing effect on soil As, the effective As content in the soil was 0.207 mg / kg, and the effective As content in the soil was reduced by 22.7%.

[0041] The above description is only a preferred embodiment of the present invention and does not limit the present invention in other forms. Any technician familiar with the profession may use the technical content disclosed above to change or modify it into an equivalent embodiment with equivalent changes and apply it to other fields. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A material for remediating arsenic-contaminated soil. It is characterized in that Includes the following ingredients: 50-70 parts of iron-modified bamboo charcoal; Humic acid 10 to 20 parts; 20 to 30 parts of iron-modified pyrolytic manganese slag.

2. The method for preparing the arsenic contaminated soil remediation material according to claim 1, It is characterized in that The following steps are involved: a. First, the alpine bamboo is dried at 80°C, and then the dried alpine bamboo is added into a quartz crucible and placed into a tubular furnace. After nitrogen is introduced, it is heated to 1000°C for 30 minutes to obtain bamboo charcoal for standby use; b. Then, the bamboo charcoal is crushed and passed through a 100-mesh sieve to obtain bamboo charcoal particles. Then, the bamboo charcoal particles are added to a potassium hydroxide solution and stirred evenly to activate the solution. c. Then, continue to add ferric nitrate to the potassium hydroxide solution and continue stirring until a red precipitate is produced; d. Then dilute with water, transfer to an oven and keep at 70°C for 60 hours, then stand at room temperature for 12 hours, wash, filter, dry, and dry to constant weight to obtain iron-modified bamboo charcoal. spare; e. Then, the manganese slag was ground and passed through a 100-mesh sieve. After drying, it was added to the FeCl3 solution and mixed. The mixture was stirred for 2 h using a magnetic stirrer. After standing for 12 h, the mixture was filtered and rinsed with deionized water until the filtrate was clear. The mixture was then dried in an oven at 105°C for later use. f. Then, the dried manganese slag is added into a quartz crucible and placed into a tubular furnace. After nitrogen is introduced, the mixture is heated to 500° C. for 30 min to obtain iron-modified pyrolytic manganese slag for standby use. g. Finally, add ultrapure water to moisten the humic acid, iron-modified bamboo charcoal, and iron-modified pyrolytic manganese slag, mix them thoroughly, and dry them at 80°C to constant weight. The desired arsenic-contaminated soil remediation material can be obtained.

3. The method for preparing the arsenic contaminated soil remediation material according to claim 2, It is characterized in that In the step c, the mass ratio of bamboo charcoal particles to ferric nitrate is 1:1.