Blast furnace low-carbon ironmaking method and device based on converter gas and coke oven gas reforming
By pretreatment and heating mixing of converter gas and coke oven gas, catalytic reaction is carried out using catalysts to generate reformed gas, which solves the problems of low utilization rate and high carbon emissions in blast furnace ironmaking process, and achieves efficient carbon emission reduction and improve economic benefits.
Patent Information
- Application Number
- CN202410872548.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing blast furnace ironmaking process, the utilization rate of converter gas and coke oven gas is low and the process is complicated, resulting in high carbon emissions and failure to fully utilize the reducing properties of H2 and CO in the gas.
By pretreating the converter gas, pressurized heating is performed with the coke oven gas, catalytic reaction is carried out under the action of the catalyst to generate reformed gas, and spray it into the blast furnace, reducing carbon deposit generation by using the catalyst's anti-carbon deposit properties .
The utilization coefficient of blast furnace is improved, carbon emissions are reduced, the reduction properties of H2 and CO in the gas are fully utilized, and some solid fuels are replaced, economic benefits are improved, and CO2 recycling is realized.
Smart Images

Figure CN118932126A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgical process, and in particular relates to a blast furnace low-carbon ironmaking method and device based on reforming converter gas and coke oven gas. Background Art
[0002] The steel industry accounts for 16% of the total energy consumption and 73% of CO2 emissions, while blast furnaces account for 70% of the energy consumption and 52% of CO2 emissions in the steel industry. Therefore, the main part of pollution reduction and carbon reduction in steel enterprises lies in the ironmaking process. To this end, it is necessary to control the source, improve the energy structure of steel enterprises, and take low-carbon production and technological innovation as the guide to improve the utilization efficiency of secondary energy in the steel production process, thereby reducing the emission pressure of steel enterprises, achieving the ultimate energy efficiency, and achieving the purpose of carbon reduction and cost reduction.
[0003] The blast furnace ironmaking process consumes a large amount of coke and coal to provide heat and reducing agents for the smelting process. In order to reduce carbon emissions from the source, some companies have explored the injection of natural gas or coke oven gas into blast furnaces. The natural gas injection system of the No. 1 blast furnace in Baoshan Base has a natural gas injection volume of 60-65Nm 3 / tHM, the solid fuel ratio dropped from 492kg / tHM to 440kg / tHM, a decrease of about 10%. The injection volume of coke oven gas at Jigang was 62.45Nm 3 / tHM, the coke ratio was reduced by 5.28kg / tHM, and the coal ratio was reduced by 40.63kg / tHM, both of which achieved good results. However, due to economic reasons and other reasons, this technology has not been widely promoted. Some companies have also conducted experimental research on blast furnace converter gas injection, but the injection process is more complicated, with gas deoxidation, carbon dioxide removal, nitrogen removal and other devices, and the investment cost is relatively high.
[0004] Smelting one ton of steel can produce 120-150Nm 3 Converter gas, the total annual output of converter gas exceeds 100 billion Nm 3 The total amount of carbon dioxide in the gas exceeds 15 billion Nm 3 ; China's coking industry produces about 191.6 billion m 3Coke oven gas, coke oven gas contains a large amount of H2 and CO, with H2 volume fraction of 55-65% and CO volume fraction of 5-10%. For a long time, converter gas and coke oven gas have been mainly used as fuel, only the calorific value of gas has been used, but the reducing property of H2 and CO has not been fully utilized, and chemical energy has not been fully utilized, which is undoubtedly a waste of resources. The current blast furnace converter gas injection process is generally divided into two categories. One is direct injection of converter gas. Since converter gas contains more CO2, CO2 injected into the blast furnace hinders the reduction of iron oxides, resulting in the inability to inject a large amount of gas, and the solid fuel substitution is relatively low; the other is to remove O2 system, CO2 system, N2 system and other systems from converter gas, which have complex processes and high investment costs, and the removed CO2 is not used and discharged into the atmosphere, and CO2 recycling cannot be achieved.
[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0006] In order to solve the technical problems of complex process flow, low utilization rate and high carbon emission of conventional converter gas and coke oven gas in the prior art, a blast furnace low-carbon ironmaking method and device based on reforming of converter gas and coke oven gas is provided.
[0007] The present invention provides a blast furnace low-carbon ironmaking method based on reforming converter gas and anxious coal gas, comprising:
[0008] Pre-treating converter gas to obtain high calorific value gas;
[0009] The high calorific value coal gas is mixed with coke oven gas to obtain a mixed gas, and the mixed gas is pressurized and heated to produce a reformed coal gas after a catalytic reaction under the action of a catalyst;
[0010] The reformed coal gas is injected into a blast furnace.
[0011] In some embodiments, the volume fractions of the components of the converter gas are: CO 55%-65%, CO2 10%-25%, N2 10%-25%, O2 0.5%-3%, H2 1%-4%; and / or, the volume fractions of the components of the coke oven gas are: H2 55%-65%, CH4 20%-28%, CO 5%-8%, CO2 2%-5%, O2 0-2%, N2 3%-6%;
[0012] Moreover, the total hydrocarbon content of the coke oven gas is less than 200 mg / Nm 3 , total sulfur content <10mg / Nm 3 .
[0013] In some embodiments, the volume ratio of the coke oven gas to the high calorific value coal gas is 1.2:1 to 1:1.6;
[0014] And / or, the volume fractions of the components of the mixed gas are: H2: 25% to 35%, CH4: 9% to 15%, CO: 28% to 38%, CO2: 8% to 18%, O2: 0 to 2%, and N2: 5% to 15%.
[0015] In some embodiments, the mixed gas is pressurized to 0.6-0.8 MPa, the pressurization frequency is 5-50 Hz, and the mixed gas is heated to a temperature of 800-1050°C.
[0016] In some embodiments, the catalyst is a Ni-based anti-carbon deposition catalyst, and the Ni-based anti-carbon deposition catalyst contains a rare earth metal oxide; preferably, the rare earth metal oxide is La2O3 or CeO2; more preferably, the rare earth metal oxide content is 0.5% to 5% of the mass of the Ni-based anti-carbon deposition catalyst. The Ni-based anti-carbon deposition catalyst has high activity, high stability and anti-carbon deposition performance. The addition of rare earth metal oxides such as La2O3 or CeO2 increases the catalyst's elimination rate of carbon deposition through its strong oxygen storage capacity, thereby inhibiting the generation of carbon deposition.
[0017] In some embodiments, the amount of reformed coal gas injected into the blast furnace is 100-500 Nm 3 / tIron.
[0018] The second aspect of the present invention provides a blast furnace low-carbon ironmaking device based on the reforming of converter gas and coke oven gas, characterized in that it comprises:
[0019] The converter gas pretreatment device comprises a spray tower and an electrostatic precipitator connected in sequence, wherein the spray tower inlet is connected to the converter outlet through a vaporization cooling flue, and the electrostatic precipitator outlet is connected to other users and the converter gas holder through an induced draft fan and a switching station;
[0020] The reforming device comprises a compressor, a heat exchanger and a reforming furnace connected in sequence, the converter gas holder and the coke oven gas pipeline are connected in parallel to the compressor inlet, the compressor outlet is connected to the reforming furnace inlet through a mixed gas pipeline, and the mixed gas pipeline passes through the heat exchanger;
[0021] The reforming furnace outlet is connected to the blast furnace inlet through a gas lance, and the blast furnace top outlet is connected to the reforming furnace burner inlet.
[0022] In some embodiments, a combustion-supporting blower and a chimney are further included, wherein the combustion-supporting blower is connected to the inlet of the reforming furnace burner through a combustion-supporting blower duct, and the combustion-supporting blower duct passes through the heat exchanger;
[0023] And / or, the hot flue gas outlet of the reformer is connected to the flue gas inlet of the heat exchanger, and the flue gas outlet of the heat exchanger is connected to the chimney.
[0024] In some embodiments, the blast furnace low-carbon ironmaking method based on the above device includes:
[0025] The converter gas is cooled and purified after passing through the vaporization cooling flue, spray tower and electrostatic precipitator in sequence;
[0026] After the converter gas is purified, it passes through the induced draft fan and the switching station in sequence, and the high calorific value gas obtained enters the converter gas tank, and the low calorific value gas enters other users;
[0027] The high calorific value gas in the converter gas tank and the coke oven gas in the coke oven gas network are connected in parallel to the compressor, and the pressurized mixed gas is preheated by the heat exchanger and enters the reactor of the reforming furnace, where a reforming reaction occurs, and the reformed gas is sprayed into the blast furnace through a gas spray gun;
[0028] The blast furnace top gas is introduced into the reforming furnace burner to heat the reforming furnace. The waste flue gas after radiation heat transfer enters the heat exchanger for waste heat recovery and is finally discharged into the atmosphere through the chimney.
[0029] In some embodiments, the induced draft fan is used to pressurize the converter gas to 2-15KPa. The switching station is provided with a CO concentration detector and a valve group. When the CO detector detects a concentration ≥60%, the valve leads to the gas tank, and when it is <60%, the valve leads to other users.
[0030] The working principle of the present invention is:
[0031] Under the action of catalyst and high temperature, the mixed gas mainly undergoes the following three reactions:
[0032] CH4+CO2=2CO +2H2 Δ r G1= 103658.892-285.92T (1)
[0033] CO2+H2=CO +H2O Δ r G2=18431.368-33.28T (2)
[0034] CH4=C (s) +2H2 Δ r G3= 86250-107.64T (3)
[0035] In the above reaction formula, T = (800-1050) + 273.15K.
[0036] Under the high temperature condition of 800~1050℃ in the reforming furnace 13, Δr G<0, all three reactions can occur. Reaction (1) is a strongly endothermic reaction and a volume-enhancing reaction. High temperature and relatively low pressure are conducive to the reforming reaction. Reaction (2) is a side reaction of the reforming reaction. When the temperature is higher than 860°C, the binding ability of H2 and O is stronger. Reaction (3) is a carbon deposition reaction, which is the main cause of catalyst deactivation, pipeline blockage and low product gas yield. H2 and H2O in the reforming gas have a certain inhibitory effect on the carbon deposition reaction. The increase of H2 promotes the reverse reaction of reaction equation (3) and reduces carbon deposition. H2O mainly reacts with carbon deposits and is conducive to the elimination of carbon deposits. In addition, CO2 is the main reactant. An increase in its concentration is conducive to the reaction with CH4 and reduces the carbon deposition of CH4. However, as CO2 increases, CH4 also needs to increase accordingly to ensure the reforming rate. Therefore, excess CO2 is removed, and anti-carbon deposition catalysts such as La2O3-Ni / MgAl2O4 can be selected. Due to the presence of higher positive valence lanthanum in the catalyst, the electrons on the surface of the metal nickel of the reduced catalyst migrate to the lanthanum; the electron concentration of the reduced metal particles decreases, which reduces the rates of CO disproportionation and methane decomposition reactions on the catalyst, thereby making the catalyst exhibit stronger anti-carbon deposition ability and reducing carbon deposition in the furnace tubes.
[0037] Compared with the prior art, the technical effects achieved by the present invention are as follows:
[0038] (1) The present invention reforms converter gas and coke oven gas to convert CH4 and CO2 into CO and H2 with high reduction potential, thereby utilizing the carbon in the converter gas and improving the blast furnace utilization factor, replacing part of the solid fuel, reducing carbon emissions, and improving economic benefits. Using the above-mentioned reformed gas as the reducing gas for blast furnace smelting can improve the gas flow distribution in the blast furnace, improve the reduction kinetic conditions in the blast furnace, increase the indirect reduction degree, reduce the solid fuel consumption of the blast furnace, achieve the goals of carbon reduction and efficiency improvement, and overcome the shortcomings of the prior art that CO2 cannot be recycled.
[0039] (2) In the prior art, converter gas and coke oven gas are mainly used as fuel, which only utilizes the calorific value of the gas, but does not fully utilize the reducing properties of H2 and CO. The present application reforms the CO2 and CH4 in the converter gas and coke oven gas, and injects the obtained CO and H2 into the blast furnace together with the original CO and H2 in the converter gas and coke oven gas to quickly reduce the iron oxides, which not only reduces carbon emissions, but also fully utilizes the reducing properties of CO and H2 in the converter gas and coke oven gas.
[0040] (3) A gas compressor is installed to provide stable, pressure-controlled gas according to the blast furnace conditions.
[0041] (4) The reforming furnace can not only reform the coal gas, but also heat the mixed gas, thereby compensating for the heat of the furnace and reducing fuel consumption.
[0042] (5) The method and device are not affected by the layout of the on-site workshop, fully utilize the existing equipment, occupy a small area, require little investment, do not need to modify the existing converter gas system, and the modification cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a blast furnace low-carbon ironmaking device and a process flow diagram of reforming converter gas and coke oven gas provided by the present invention;
[0044] In the figure: 1-converter, 2-vaporization and cooling flue, 3-spray tower, 4-electrostatic precipitator, 5-induced draft fan, 6-switching station, 7-other users, 8-converter gas holder, 9-coke oven gas pipeline network, 10-pressurizer, 11-heat exchanger, 12-chimney, 13-combustion-supporting fan, 14-reforming furnace, 15-gas spray gun, 16-blast furnace. DETAILED DESCRIPTION
[0045] The technical solution of the present invention is described below by specific embodiments in conjunction with the accompanying drawings. It should be understood that one or more steps mentioned in the present invention do not exclude the existence of other methods and steps before and after the combination step, or other methods and steps can be inserted between these explicitly mentioned steps. It should also be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. Unless otherwise specified, the numbering of each method step is only for the purpose of identifying each method step, and is not intended to limit the order of arrangement of each method or to define the scope of implementation of the present invention. Changes or adjustments in their relative relationships can also be regarded as the scope of implementation of the present invention without substantial changes in the technical content.
[0046] The sources of the raw materials and instruments used in the examples are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0047] like Figure 1 As shown, a blast furnace low-carbon ironmaking device based on the reforming of converter gas and coke oven gas includes: a converter gas pretreatment device, a reforming device and a blast furnace.
[0048] The converter gas pretreatment device comprises a spray tower 3 and an electrostatic precipitator 4 which are connected in sequence. The inlet of the spray tower 3 is connected to the outlet of the converter 1 through a vaporization cooling flue 2. The outlet of the electrostatic precipitator 4 is connected to other users 7 and a converter gas holder 8 through an induced draft fan 5 and a switching station 6.
[0049] The reforming device comprises a compressor 10, a heat exchanger 11 and a reforming furnace 14 connected in sequence, the converter gas holder 8 and the coke oven gas pipeline 9 are connected in parallel to the inlet of the compressor 10, the outlet of the compressor 10 is connected to the inlet of the reforming furnace 14 through a mixed gas pipeline, and the mixed gas pipeline passes through the heat exchanger 11;
[0050] The reforming furnace 14 outlet is connected to the blast furnace 16 inlet via a gas lance 15 , and the blast furnace 16 top outlet is connected to the reforming furnace 14 burner inlet.
[0051] In some embodiments, a combustion-supporting fan 13 and a chimney 12 are further included, wherein the combustion-supporting fan 13 is connected to the burner inlet of the reforming furnace 14 through a combustion-supporting air duct, and the combustion-supporting air duct passes through the heat exchanger 11;
[0052] And / or, the hot flue gas outlet of the reformer is connected to the flue gas inlet of the heat exchanger, and the flue gas outlet of the heat exchanger is connected to the chimney.
[0053] In some embodiments, the radiation convection chamber of the reforming furnace 14 is built with refractory materials that are resistant to high temperatures and gas erosion, and a high-temperature resistant furnace tube is arranged in the furnace, and a Ni-based anti-carbon deposition catalyst is arranged in the furnace tube. Rare earth metal oxides La2O3 or CeO2 are added to the Ni-based anti-carbon deposition catalyst. The mixed gas is heated to above 850°C in the radiation convection chamber, and a CH4-CO2 reforming reaction occurs to produce high reduction potential coal gas. Convection finned tubes are arranged in the heat exchanger 14 to preheat the combustion-supporting air and the mixed gas of high calorific value coal gas and coke oven gas.
[0054] The low-carbon ironmaking method using the blast furnace low-carbon ironmaking device based on the reforming of converter gas and coke oven gas comprises:
[0055] (1) Pretreatment of converter gas: The converter gas released from the outlet of the converter 1 passes through the vaporization cooling flue 2, the spray tower 3 and the electrostatic precipitator in sequence to achieve cooling and purification of the converter gas. The purified converter gas is pressurized to 2-15Kpa by the induced draft fan 5 and enters the switching station 6. The switching station 6 is equipped with a CO concentration detector and a valve group. When the CO detector detects a concentration of ≥60%, it is high calorific value gas, and the valve leads to the converter gas tank 8. When it is less than 60%, the valve leads to other users 7.
[0056] (2) Reforming: The high calorific value coal gas is mixed with the coke oven gas in the coke oven gas network 9 to obtain a mixed coal gas. The mixed coal gas is pressurized to 0.6-0.8 MPa by a compressor 10 at a frequency of 5-50 Hz to ensure that a stable and pressure-controlled mixed coal gas is provided to the blast furnace injection system. After the pressurized mixed coal gas enters the reforming furnace 14, a reforming reaction occurs under the action of a high temperature of 800-1050°C and a Ni-based anti-carbon deposition catalyst with rare earth metal oxides added. The obtained reformed gas enters the blast furnace 16 through a gas injection gun 15. The amount of reformed gas injected into the blast furnace is 100-500 Nm 3 / t iron, each injection 1Nm 3 The ratio of reformed gas to solid fuel is 0.2-0.4 kg / t.
[0057] Furthermore, the temperature of the mixed gas at the outlet of the compressor 10 is 50-150°C, and after heat exchange in the heat exchanger 11, the temperature of the mixed gas reaches 500-650°C.
[0058] Furthermore, the temperature of the combustion-supporting air at the outlet of the combustion-supporting fan 13 is 30-100°C, and after heat exchange in the heat exchanger 11, the temperature of the combustion-supporting air at the outlet is 200-400°C.
[0059] Furthermore, after the mixed coal gas enters the reforming furnace 14, the temperature is heated to 800-1050°C. The heat required by the reforming furnace 14 comes from part of the top gas generated by the blast furnace 16 and the heat generated by the combustion of preheated air. A dry reforming catalyst is arranged in the furnace tube of the reforming furnace 14. Under the action of the catalyst and high temperature, the mixed coal gas undergoes a reforming reaction.
[0060] Furthermore, the temperature of the waste flue gas at the outlet of the reforming furnace 14 is 750-1150°C, and waste heat is recovered in the heat exchanger 11. The heat exchanger 11 is provided with a steam waste heat recovery section. The temperature of the waste flue gas entering the chimney 12 after heat exchange is <200°C, and the heat of the flue gas is effectively utilized.
[0061] In some embodiments, the volume fractions of the components of the converter gas are: CO 55% to 65%, CO2 10% to 25%, N2 10% to 25%, O2 0.5% to 3%, H2 1% to 4%;
[0062] And / or, the volume fractions of the components of the coke oven gas are: H2 55% to 65%, CH4 20% to 28%, CO 5% to 8%, CO2 2% to 5%, O2 0% to 2%, N2 3% to 6%;
[0063] Moreover, the total hydrocarbon content of the coke oven gas is less than 200 mg / Nm 3 , total sulfur content <10mg / Nm 3 .
[0064] In some embodiments, the volume ratio of the coke oven gas to the high calorific value gas is 1.2:1 to 1:1.6;
[0065] The volume fractions of the components of the mixed gas are: H2: 25% to 35%, CH4: 9% to 15%, CO: 28% to 38%, CO2: 8% to 18%, O2: 0 to 2%, and N2: 5% to 15%.
[0066] The above-mentioned blast furnace low-carbon ironmaking method based on the reforming of converter gas and coke oven gas automatically separates, stores and transports the high calorific value converter gas, mixes it with the coke oven gas and pressurizes it, and then enters the reforming furnace for dry reforming, and finally is sprayed into the blast furnace through a gas spray gun. The reformed gas rich in CO and H2 is quickly heated in the vortex zone of the tuyere, and then enters the upper indirect reduction zone to reduce the iron oxides, thereby improving the indirect reduction rate and solving the problems of low theoretical combustion temperature of the tuyere and decreased coal powder combustion rate in the process of directly injecting converter gas and / or coke oven gas into the blast furnace. Moreover, this part of CO and H2 replaces the CO generated by the combustion of coke before the tuyere, can replace part of the coke, reduce the coke consumption, and reduce the total CO2 emissions of the ironmaking process.
[0067] The reforming medium is not limited to the reforming of converter gas and coke oven gas. The reforming of converter gas and natural gas into the blast furnace injection system is also within the scope of protection of this patent. The mixing ratio of natural gas and converter gas is 1:6~1:4, and the volume fractions of each component of the mixed gas are: H2: 1%~2%, CH4: 10%~20%, CO: 45%~55%, CO2: 15%~20%, O2: 0~1%, N2: 12%~17%.
[0068] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A blast furnace low-carbon ironmaking method based on reforming converter gas and coke oven gas, characterized in that: include: Pre-treating converter gas to obtain high calorific value gas; The high calorific value coal gas is mixed with coke oven gas to obtain a mixed gas, and the mixed gas is pressurized and heated to produce a reformed coal gas after a catalytic reaction under the action of a catalyst; The reformed coal gas is injected into a blast furnace.
2. The blast furnace low-carbon ironmaking method based on reforming converter gas and coke oven gas according to claim 1, characterized in that: The volume fractions of the components of the converter gas are: CO 55% to 65%, CO2 10% to 25%, N2 10% to 25%, O2 0.5% to 3%, H2 1% to 4%; And / or, the volume fractions of the components of the coke oven gas are: H2 55% to 65%, CH4 20% to 28%, CO 5% to 8%, CO2 2% to 5%, O2 0% to 2%, N2 3% to 6%; Moreover, the total hydrocarbon content of the coke oven gas is less than 200 mg / Nm 3 , total sulfur content <10mg / Nm 3 .
3. The blast furnace low-carbon ironmaking method based on reforming converter gas and coke oven gas according to claim 1, characterized in that: The volume ratio of the coke oven gas to the high calorific value gas is 1.2:1 to 1:1.6; And / or, the volume fractions of the components of the mixed gas are: H2: 25% to 35%, CH4: 9% to 15%, CO: 28% to 38%, CO2: 8% to 18%, O2: 0 to 2%, and N2: 5% to 15%.
4. The blast furnace low-carbon ironmaking method based on reforming converter gas and coke oven gas according to claim 1, characterized in that: The mixed gas is pressurized to 0.6-0.8 MPa, with a pressurization frequency of 5-50 Hz, and heated to a temperature of 800-1050°C.
5. The blast furnace low-carbon ironmaking method based on reforming converter gas and coke oven gas according to claim 1, characterized in that: The catalyst is a Ni-based anti-carbon deposition catalyst, and the Ni-based anti-carbon deposition catalyst contains rare earth metal oxide; preferably, the rare earth metal oxide is La2O3 or CeO2; more preferably, the rare earth metal oxide content is 0.5% to 5% of the mass of the Ni-based anti-carbon deposition catalyst.
6. The blast furnace low-carbon ironmaking method based on reforming converter gas and coke oven gas according to claim 1, characterized in that: The amount of reforming gas injected into the blast furnace is 100-500 Nm 3 / tIron.
7. A blast furnace low-carbon ironmaking device based on reforming converter gas and coke oven gas, characterized in that: include: The converter gas pretreatment device comprises a spray tower and an electrostatic precipitator connected in sequence, wherein the spray tower inlet is connected to the converter outlet through a vaporization cooling flue, and the electrostatic precipitator outlet is connected to other users and the converter gas holder through an induced draft fan and a switching station; The reforming device comprises a compressor, a heat exchanger and a reforming furnace connected in sequence, the converter gas holder and the coke oven gas pipeline are connected in parallel to the compressor inlet, the compressor outlet is connected to the reforming furnace inlet through a mixed gas pipeline, and the mixed gas pipeline passes through the heat exchanger; The reforming furnace outlet is connected to the blast furnace inlet through a gas lance, and the blast furnace top outlet is connected to the reforming furnace burner inlet.
8. The blast furnace low-carbon ironmaking device based on reforming converter gas and coke oven gas according to claim 7, characterized in that: It also includes a combustion-supporting fan and a chimney, wherein the combustion-supporting fan is connected to the inlet of the reforming furnace burner through a combustion-supporting air duct, and the combustion-supporting air duct passes through the heat exchanger; And / or, the hot flue gas outlet of the reformer is connected to the flue gas inlet of the heat exchanger, and the flue gas outlet of the heat exchanger is connected to the chimney.
9. The ironmaking method using reformed coal gas in a blast furnace low-carbon ironmaking device according to claim 7 or 8, characterized in that: include: The converter gas is cooled and purified after passing through the vaporization cooling flue, spray tower and electrostatic precipitator in sequence; After the converter gas is purified, it passes through the induced draft fan and the switching station in sequence, and the high calorific value gas obtained enters the converter gas tank, and the low calorific value gas enters other users; The high calorific value gas in the converter gas tank and the coke oven gas in the coke oven gas network are connected in parallel to the compressor, and the pressurized mixed gas is preheated by the heat exchanger and enters the reactor of the reforming furnace, where a reforming reaction occurs, and the reformed gas is sprayed into the blast furnace through a gas spray gun; The blast furnace top gas is introduced into the reforming furnace burner to heat the reforming furnace. The waste flue gas after radiation heat transfer enters the heat exchanger for waste heat recovery and is finally discharged into the atmosphere through the chimney.
10. The ironmaking method according to claim 9, characterized in that: The induced draft fan is used to pressurize the converter gas to 2-15KPa. The switching station is provided with a CO concentration detector and a valve group. When the CO detector detects a concentration ≥60%, the valve leads to the gas tank, and when <60%, the valve leads to other users.
Citation Information
Cited By
Method and system for preparing synthesis gas from coke oven gas and over-limit converter gas
CN121449019A