Production method of tellurium-containing sulfur-containing steel
By controlling the activity and temperature of the liquid steel, combined with the staged feeding of tellurium core-containing wire and bottom-blown argon stirring technology, the problem of low tellurium yield is solved, and a high and stable tellurium yield and cost is achieved. Reduction ensures efficient processing performance of sulfur-containing steel.
Patent Information
- Application Number
- CN202411017343.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has low yield and unstable during the process of liquid steel smelting, resulting in high production costs of high-end tellurium-containing special steels, and poor uniform distribution of tellurium in the steel, affecting material performance.
By controlling the oxygen activity and temperature of the steel liquid, combined with the method of feeding the tellurium core-containing wire in segments, we ensure that the tellurium is evenly distributed in the steel liquid. The carbonized rice husk is covered with bottom-blown argon gas stirring and post-treatment to improve the Receiving rate and stability.
The tellurium yield rate is not less than 75%, and the production cost is reduced, ensuring the uniform distribution and efficient processing performance of tellurium in sulfur-containing steel.
Smart Images

Figure BDA0004966145320000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of iron and steel metallurgy, and relates to a method for producing tellurium-containing and sulfur-containing steel, and in particular to a method for producing tellurium-containing and sulfur-containing steel by a converter-refining-continuous casting process and improving the tellurium yield. Background Art
[0002] In order to improve the morphology and distribution of sulfides in sulfur-containing special steels, make them have good cutting performance, and meet the needs of mechanical processing users for efficient processing, a certain amount of tellurium can be added to the sulfur-containing steel, and tellurium can be used to modify the sulfides. Tellurium coexists with sulfides in steel, which can optimize the morphology of sulfides, improve the rating, reduce magnetic trace defects, and improve the cutting performance of materials. Tellurium can regulate the type of sulfides, modify rod-shaped sulfides into ellipsoidal sulfides, avoid deformation of sulfides into long strips along the rolling direction, and improve the sulfide rating. Tellurium is widely used in the production of free-cutting steel, gear steel, mold steel, etc. By controlling the appropriate amount of tellurium added and the tellurium-sulfur ratio, the performance of sulfur-containing steel products can be improved, and high-end tellurium-containing special steels can be developed.
[0003] Tellurium and sulfur are in the same main group and have similar properties. The two cannot form compounds, but they are miscible in the molten state. At room temperature, tellurium does not react with water, oxygen, or non-oxidizing acids, and has good chemical stability; at high temperatures, tellurium can react with water to produce hydrogen and TeO2. Tellurium does not burn when heated in air, but produces TeO2 and a blue-green flame. The melting point of tellurium is 452°C and the boiling point is 1390°C, both of which are lower than the steelmaking temperature. Directly adding tellurium to steel will easily evaporate and sublimate, resulting in a low yield. How to ensure that the expensive tellurium can be added to steel with a high yield is the key to the development of high-end tellurium-containing special steels.
[0004] CN 107841595A discloses a tellurium-containing cored wire, which is composed of a core material and a low-carbon steel cored tube, wherein the core material is composed of a mixture of tellurium and sulfur and inevitable impurities. During the refining of molten steel, the tellurium-containing cored wire is added to the molten steel as an alloy material to modify the inclusions in the sulfur-containing steel. However, the patent does not specify the tellurium yield of cored wires with core materials of different components under the same process, and it is impossible to determine the core material composition when the tellurium yield is higher.
[0005] CN 106756635 A discloses a method for preparing tellurium-containing steel and the tellurium-containing steel. The steps of adding tellurium to the molten steel include the following aspects: using steel skin to wrap tellurium to make tellurium powder cored wire, using a mobile wire feeder to feed the wire, the feeding position is above the bottom blowing argon hole, the bottom blowing argon is stirred, and the bottom blowing argon flow rate is 50-700Nm3 / min. After the wire feeding is completed, the bottom blowing argon is continued for 5-20 minutes, and the bottom blowing argon flow rate is 100-200Nm3 / min. Under the process conditions provided by the patent, the tellurium recovery rate is 50%-70%, but the patent adopts one-time feeding of all the cored wires, which will lead to excessive concentration of alloy elements in the local molten steel, serious element volatilization and easy to cause segregation problems.
[0006] CN 110117693A discloses a tellurium-adding process for tellurium-containing free-cutting steel, wherein the oxygen activity of the steel liquid is controlled to be 5-50ppm when tellurium is added at the end of refining, the temperature of the steel liquid is 50-75℃ above the liquidus temperature, and the thickness of the slag layer is not less than 1cm; the tellurium-containing cored wire is intermittently fed into the steel liquid at least three times by an intermittent wire feeding method, the wire feeding speed is 60-150m / min, the time interval is 10-20s, and the argon flow rate of the bottom blowing argon is 100-300NL / min; after the wire feeding is completed, the surface of the steel liquid is covered with carbonized rice husks, and soft argon blowing and stirring are continued at an argon flow rate of 100-180NL / min. After the composition and temperature reach the finished product process requirements of the target steel liquid, the subsequent ladle tapping process is carried out. Under the process conditions provided by the patent, the tellurium recovery rate is greater than 65%, the patent process has a large operating window range, and the tellurium recovery rate is unstable.
[0007] CN 114908216A discloses a method for adding bismuth and tellurium to free-cutting steel, free-cutting carburized steel and its application, and provides a method for adding bismuth and tellurium to free-cutting steel: at the end of molten steel refining, after the adjustment of other components except bismuth and tellurium is completed, tellurium source and bismuth source are sprayed to the bottom of molten steel by compressed inert gas to prepare free-cutting molten steel containing bismuth and tellurium. Under the process conditions provided in the patent, the measured yield is greater than 85%, but the timing of tellurium addition is not clear, and the tellurium yield is unstable.
[0008] The above methods provide industrial methods for adding tellurium from different perspectives, but they all have certain limitations. Summary of the invention
[0009] The purpose of the present invention is to overcome the shortcomings of the above-mentioned existing technologies and provide a method for producing tellurium-containing and sulfur-containing steel. The method uses comprehensive means to control the oxygen activity and the temperature of the molten steel within the optimal range to improve the yield of stable tellurium and make the tellurium evenly distributed in the molten steel, thereby ultimately obtaining good inclusions while reducing production costs.
[0010] To achieve the above object, the technical solution of the present invention is:
[0011] A method for producing tellurium-containing and sulfur-containing steel, the process flow is converter → LF furnace refining → VD / RH furnace refining → continuous casting / mold casting, characterized in that: the chemical composition weight percentage of the steel is: C=0.05-0.49%, Si=0.01-1.2%, Mn=0.60-1.60%, P≤0.025%, S=0.02-0.36%, V=0.08-1.20%, Cr≤0.3%, Mo≤0.08%, N=0.01-0.02%, Al≤0.02%, O≤0.0025%, Te=0.0001-0.008%, 0.075[S]≤Te≤0.0045%; the rest is Fe and unavoidable impurity elements; the key process steps include:
[0012] 1) Molten steel refining: At the end of the molten steel refining, after the adjustment of other components except tellurium is completed, argon is blown at the bottom for full stirring for 3 to 5 minutes, and the argon flow rate of the bottom blowing argon is 150 to 300 NL / min, and then tellurium-containing cored wire is added to the molten steel for alloying, and the thickness of the molten steel slag layer is controlled to be about 1.2 to 1.5 cm at this time;
[0013] 2) Tellurium feeding: Before feeding tellurium, the oxygen activity in the molten steel must be 5-40ppm. The specific oxygen activity needs to be further determined according to the target tellurium content of the steel grade. The target oxygen activity = (-0.3*target tellurium content + 27) ± 3, the unit of oxygen activity is ppm, and the unit of target tellurium content is ppm; the temperature of the molten steel is 40-45°C above the liquidus of the target production steel grade. According to the size of the ladle, the tellurium-containing cored wire is divided into several sections and fed into the ladle in sequence. The feeding position is above the bottom blowing argon hole. Each feeding is 20-30m, the interval is 10-15s, the wire feeding speed of the wire feeding machine is 2-3m / s, and argon is not blown bottom during the wire feeding process. Argon bottom blowing is performed during the interval between two feedings, and the argon flow rate of the argon bottom blowing is 120-250NL / min;
[0014] 3) Argon blowing: Bottom blowing of argon during molten steel refining can be divided into three stages: Stage 1: fine-tuning of other components except tellurium, at which time the argon flow rate of bottom blowing argon is always 150-300NL / min; Stage 2: feeding tellurium-containing cored wire, no argon bottom blowing during the feeding process, argon bottom blowing during the feeding interval, the argon flow rate of the bottom blowing argon is 120-250NL / min; Stage 3: after feeding the tellurium-containing wire, continue to blow argon at the bottom, at which time the argon flow rate of the bottom blowing argon is 100-180NL / min, and the blowing time is 10-15min;
[0015] 4) Post-processing: Optimize the post-feeding wire protection process. After feeding all tellurium-containing cored wires, post-process the obtained molten steel. Cover the surface of the molten steel with carbonized rice husks and perform bottom blowing of argon. The argon flow rate of the bottom blowing is 100-180NL / min. After the argon blowing time is 10-15min, the temperature is measured and sampled again. After the composition and temperature meet the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
[0016] Furthermore, the step 2) feeding tellurium: the core tube and core material of the tellurium-containing cored wire are composed of: the core material is a mixed component of pure tellurium powder and industrial pure iron powder, the ratio of pure tellurium powder to industrial pure iron powder is 1:(1.5~2.5), the weight of the core material per meter of the cored wire is 330~360g, and the outer diameter of the tellurium-containing cored wire is φ10~13mm; the core tube is low carbon steel with a thickness of 0.3~0.4mm.
[0017] Furthermore, in the step 2) of feeding tellurium, the wire feeding machine guide tube should be vertically inserted into the molten steel, and the outlet of the wire feeding machine guide tube should be 20 to 40 cm away from the molten steel surface.
[0018] Preferably, the sulfur-containing tellurium-containing steel is a non-quenched and tempered steel, and its composition is C=0.37%, Si=0.65%, Mn=1.00%, P=0.025%, S=0.035%, Cr=0.16%, V=0.29%, Al=0.006%, N=0.017%, O≤0.0025%, Te=0.0001-0.008% by mass percentage, and the rest are Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the molten steel temperature needs to be controlled at 1531-1536°C.
[0019] Furthermore, the sulfur-containing tellurium-containing steel is a free-cutting steel, and its chemical composition is C=0.063%, Si=0.009%, Mn=1.266%, P=0.025%, S=0.05%, Al=0.001%, O≤0.0025%, Te=0.0001-0.008% by mass percentage, and the rest is Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the molten steel temperature needs to be controlled at 1554-1559°C.
[0020] Furthermore, the sulfur-containing tellurium-containing steel is a gear steel, and its composition by mass percentage is C=0.19%, Si: 0.08%, Mn=1.3%, P: 0.022%, S=0.028%, Cr=1.18%, Al=0.039%, O≤0.0025%, Te=0.0001-0.008%, and the rest is Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the molten steel temperature needs to be controlled at 1533-1538°C.
[0021] The oxygen activity needs to be further determined according to the target tellurium content of the steel grade, target oxygen activity = (-0.3*target tellurium content + 27) ± 3, the unit of oxygen activity is ppm, and the unit of target tellurium content is ppm;
[0022] The tellurium recovery rate has the following relationship with the tellurium content, oxygen activity and temperature of the molten steel: Tellurium recovery rate = 100 + (-930·tellurium content·(1-(oxygen activity-15) 2 / 625)) / molten steel temperature ±2, tellurium yield in %, tellurium content in ppm, oxygen activity in ppm, molten steel temperature in K;
[0023] The innovation of the present invention is as follows: First, the present invention finds that the tellurium yield is related to the tellurium content, oxygen activity and molten steel temperature of the steel during the smelting process, and proposes the relationship therein. By integrating the existing process means, the oxygen activity and molten steel temperature during the smelting process are accurately controlled, and the mathematical relationship between the oxygen activity and the target tellurium content is proposed, thereby improving and stabilizing the tellurium yield while ensuring the target tellurium content; Second, the method of the present invention is to improve and stabilize the tellurium yield of tellurium-containing and sulfur-containing steel during the production process, rather than the means of adding tellurium, but the means of adding tellurium is indeed a necessary technology for the realization of this technology. The innovation of this technology lies in the relationship between the tellurium yield and the tellurium content, oxygen activity and molten steel temperature. By finely controlling the tellurium content, oxygen activity and molten steel temperature, a high and stable yield is achieved. Therefore, the beneficial effects of the present invention include: the tellurium modification process is clear, the details are clear, and the operability is strong; the tellurium recovery rate of the sulfur-containing steel after tellurium modification is not less than 75%, and the tellurium recovery rate is high and stable; the production cost of the tellurium-modified sulfur-containing steel is low, the morphology of Class A inclusions in the sulfur-containing steel is good, and the rating is improved. DETAILED DESCRIPTION
[0024] The technical solution of the present invention is described in detail below through examples. The following examples are only used to explain and illustrate the technical solution of the present invention, and cannot be interpreted as limiting the technical solution of the present invention.
[0025] Embodiment 1:
[0026] This embodiment provides a tellurium-modified non-quenched and tempered steel, whose main components (wt%) are: C: 0.37%, Si: 0.65%, Mn: 1.00%, P: 0.025%, S: 0.035%, Cr: 0.16%, V: 0.29%, Al: 0.006%, N: 0.017%, O≤0.0025%, Te=0.0001-0.008%, and the rest are Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the temperature of the molten steel needs to be controlled at 1531-1536°C. The smelting process flow adopted by this process is: converter → LF furnace refining → VD furnace refining → continuous casting, and the tellurium-containing cored wire with a total length of 100m is fed at the end of VD refining.
[0027] The tellurium-containing cored wire selected in this embodiment is composed of a cored tube and a core material, the cored tube is 08 steel with a thickness of 0.3 mm, the core material is a ratio of pure tellurium powder to industrial pure iron powder of 1:2.5, the core material weight of each meter of the cored wire is 360 g, and the outer diameter of the tellurium-containing cored wire is φ12 mm. The process of feeding the tellurium-containing cored wire is:
[0028] (1) At the end of molten steel refining, after the adjustment of other components except tellurium is completed, argon is blown at the bottom for full stirring for 3 to 5 minutes, the argon flow rate of the bottom blowing argon is 250 NL / min, the thickness of the molten steel slag layer is controlled to be 1.2 to 1.5 cm, the oxygen activity of the molten steel is 15 to 30 ppm, and the temperature of the molten steel is 1535° C. After the above conditions are met, tellurium-containing cored wire is fed into the steel;
[0029] (2) feeding the tellurium-containing cored wire into the ladle in four times, feeding 30, 30, 20, and 20 m respectively, with an interval of 12 s for the next feeding, the feeding position is above the bottom blowing argon hole, the outlet of the wire feeder conduit is 22 cm away from the steel liquid surface, the wire feeding speed of the wire feeder is 2.5 m / s, no bottom blowing of argon is performed during the wire feeding process, and argon bottom blowing is performed between two feedings, and the argon flow rate of the argon bottom blowing is 150 NL / min;
[0030] (3) After all the tellurium-containing cored wires are fed, the obtained molten steel is post-treated by covering the surface of the molten steel with carbonized rice husks and performing bottom blowing of argon gas. The argon flow rate of the bottom blowing is 140 NL / min. After the argon blowing time is 12 to 15 minutes, the temperature is measured and sampled again. After the composition and temperature reach the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
[0031] In the on-site production of this embodiment, the wire feeding process is stable, the reaction is gentle, and there is no violent splashing.
[0032] The tellurium content of the non-quenched and tempered steel containing tellurium prepared by the process of this embodiment is 33 ppm as measured by ICP. The tellurium recovery rate is calculated to be 83% based on the added amount.
[0033] Embodiment 2:
[0034] This embodiment is basically the same as the first embodiment, except that:
[0035] This embodiment provides a tellurium-modified free-cutting steel, the main components (wt%) of which are: C: 0.063%, Si: 0.009%, Mn: 1.266%, P: 0.025%, S: 0.05%, Al: 0.001%, O≤0.0025%, Te=0.0001-0.008%, and the rest are Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the temperature of the molten steel needs to be controlled at 1554-1559°C. The smelting process adopted by this process is: converter → LF furnace refining → continuous casting, and the tellurium-containing cored wire with a total length of 120m is fed at the end of LF refining.
[0036] The tellurium-containing cored wire selected in this embodiment is composed of a cored tube and a core material. The cored tube is 08 steel with a thickness of 0.3 mm. The core material is a ratio of pure tellurium powder to industrial pure iron powder of 1:2.5. The weight of the core material per meter of the cored wire is 360 g. The outer diameter of the tellurium-containing cored wire is φ12 mm.
[0037] The process of feeding tellurium cored wire is:
[0038] (1) At the end of the refining of the molten steel, after the adjustment of other components except tellurium is completed, argon is blown at the bottom for sufficient stirring for 5 minutes, the argon flow rate of the bottom blowing argon is 200 NL / min, the thickness of the molten steel slag layer is controlled to be 1.3 cm, the oxygen activity of the molten steel is 10 ppm, and the temperature of the molten steel is 1555° C. After the above conditions are met, tellurium-containing cored wire is fed into the steel;
[0039] (2) feeding the tellurium-containing cored wire into the ladle in four times, each time feeding 30 m, with an interval of 12 s for the next feeding, the feeding position is above the bottom blowing argon hole, the outlet of the wire feeder conduit is 25 cm away from the steel liquid surface, the wire feeding speed of the wire feeder is 2-3 m / s, no argon is blown at the bottom during the wire feeding process, and argon is blown at the bottom between two feedings, and the argon flow rate of the argon bottom blowing is 220 NL / min;
[0040] (3) After all the tellurium-containing cored wires are fed, the obtained molten steel is post-treated by covering the surface of the molten steel with carbonized rice husks and bottom blowing argon gas. The argon flow rate of the bottom blowing argon gas is 130 NL / min. After the argon blowing time is 12 to 15 minutes, the temperature is measured and sampled again. After the composition and temperature reach the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
[0041] In the on-site production of this embodiment, the wire feeding process is stable, the reaction is gentle, and there is no violent splashing.
[0042] The tellurium content of the carbon free-cutting steel produced by the tellurium-containing free-cutting steel liquid prepared by the process of this embodiment is 45 ppm as measured by ICP. The tellurium recovery rate is 78% based on the added amount.
[0043] Embodiment 3:
[0044] This embodiment is basically the same as the first embodiment, except that:
[0045] This embodiment provides a tellurium-modified gear steel, the main components (wt%) of which are: C: 0.19%, Si: 0.08%, Mn: 1.3%, P: 0.022%, S: 0.028%, Cr: 1.18%, Al: 0.039%, and the rest are Fe and unavoidable impurity elements. The smelting process adopted in this process is: electric furnace smelting → LF furnace refining → RH furnace refining → continuous casting, and a tellurium-containing cored wire with a total length of 50m is fed at the end of RH refining.
[0046] The tellurium-containing cored wire selected in this embodiment is composed of a cored tube and a core material. The cored tube is 08 steel with a thickness of 0.3 mm. The core material is a ratio of pure tellurium powder to industrial pure iron powder of 1:2.5. The weight of the core material per meter of the cored wire is 360 g. The outer diameter of the tellurium-containing cored wire is φ12 mm.
[0047] The process of feeding tellurium cored wire is:
[0048] (1) At the end of the refining of the molten steel, after the adjustment of other components except tellurium is completed, argon is blown at the bottom for full stirring for 3 minutes, the argon flow rate of the bottom blowing argon is 200 NL / min, the thickness of the molten steel slag layer is controlled to be 1.3 cm, the oxygen activity of the molten steel is 16 ppm, and the temperature of the molten steel is 1532° C. After the above conditions are met, tellurium-containing cored wire is fed into the steel;
[0049] (2) feeding the tellurium-containing cored wire into the ladle twice, feeding 25 m each time, and feeding the next time after an interval of 12 seconds. The feeding position is above the bottom blowing argon hole, the outlet of the wire feeding machine conduit is 20 to 30 cm away from the steel liquid surface, and the wire feeding speed of the wire feeding machine is 2 to 3 m / s. During the wire feeding process, argon is not blown at the bottom. Argon is blown at the bottom between two feedings. The argon flow rate of the argon bottom blowing is 120-250180 NL / min;
[0050] (3) After all the tellurium-containing cored wires are fed, the resulting molten steel is post-treated by covering the surface of the molten steel with carbonized rice husks and performing bottom blowing of argon gas. The argon flow rate of the bottom blowing is 130 NL / min. After the argon blowing time is 13 minutes, the temperature is measured and sampled again. After the composition and temperature reach the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
[0051] In the on-site production of this embodiment, the wire feeding process is stable, the reaction is gentle, and there is no violent splashing.
[0052] The tellurium content of the tellurium-containing gear steel prepared by the process of this embodiment is 201 ppm as measured by ICP. The tellurium recovery rate is calculated to be 85% based on the added amount.
[0053] Comparative Example 1:
[0054] This comparative example is basically the same as Example 1, except that:
[0055] This comparative example provides a tellurium-modified non-quenched and tempered steel, whose main components (wt%) are: C: 0.37%, Si: 0.65%, Mn: 1.00%, P: 0.027%, S: 0.036%, Cr: 0.15%, V: 0.29%, Al: 0.006%, N: 0.016%, O≤0.0025%, Te=0.0001-0.008%, and the rest are Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the temperature of the molten steel needs to be controlled at 1533-1538°C. The smelting process adopted in this process is: converter → LF furnace refining → VD furnace refining → continuous casting, and the tellurium-containing cored wire with a total length of 100m is fed at the end of VD refining.
[0056] The tellurium-containing cored wire selected in this embodiment is composed of a cored tube and a core material. The cored tube is 08 steel with a thickness of 0.5 mm, the core material is pure tellurium powder, the core material weight of each meter of the cored wire is 350 g, and the outer diameter of the tellurium-containing cored wire is φ11 mm.
[0057] The process of feeding tellurium cored wire is:
[0058] (1) At the end of the refining of the molten steel, after the adjustment of other components except tellurium is completed, argon is blown at the bottom for sufficient stirring for 3 to 5 minutes, the argon flow rate of the bottom blowing argon is 150 to 300 NL / min, the thickness of the molten steel slag layer is controlled to be 1.3 cm, the oxygen activity of the molten steel is 30 ppm, and the temperature of the molten steel is 1549° C. After the above conditions are met, tellurium-containing cored wire is fed into the steel;
[0059] (2) feeding the tellurium-containing cored wire into the ladle in four times, feeding 30, 30, 20, and 20 m respectively, with an interval of 12 s for the next feeding, the feeding position is above the bottom blowing argon hole, the outlet of the wire feeder conduit is 25 cm away from the steel liquid surface, the wire feeding speed of the wire feeder is 2-3 m / s, no argon is blown at the bottom during the wire feeding process, and argon is blown at the bottom between two feedings, and the argon flow rate of the argon bottom blowing is 180 NL / min;
[0060] (3) After all the tellurium-containing cored wires are fed, the resulting molten steel is post-treated by covering the surface of the molten steel with carbonized rice husks and performing bottom blowing of argon gas. The argon flow rate of the bottom blowing is 140 NL / min. After the argon blowing time is 13 minutes, the temperature is measured and sampled again. After the composition and temperature reach the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
[0061] In the on-site production of this embodiment, the wire feeding process is stable, the reaction is gentle, and there is no violent splashing.
[0062] The tellurium content of the carbon free-cutting steel produced by the tellurium-containing free-cutting steel liquid prepared by the process of this embodiment is 25 ppm as measured by ICP. The tellurium recovery rate is 62% based on the added amount.
[0063] Comparative Example 2:
[0064] This embodiment is basically the same as the second embodiment, except that:
[0065] This embodiment provides a tellurium-modified free-cutting steel, the main components (wt%) of which are: C: 0.064%, Si: 0.009%, Mn: 1.27%, P: 0.025%, S: 0.05%, Al: 0.0014%, and the rest are Fe and unavoidable impurity elements. The smelting process adopted in this process is: converter → LF furnace refining → continuous casting, and a tellurium-containing cored wire with a total length of 120m is fed at the end of LF refining.
[0066] The tellurium-containing cored wire selected in this embodiment is composed of a cored tube and a core material. The cored tube is 08 steel with a thickness of 0.3 mm. The core material is a ratio of pure tellurium powder to industrial pure iron powder of 1:2.5. The weight of the core material per meter of the cored wire is 360 g. The outer diameter of the tellurium-containing cored wire is φ12 mm.
[0067] The process of feeding tellurium cored wire is:
[0068] (1) At the end of steel refining, after the adjustment of other components except tellurium is completed, tellurium-containing cored wire is fed into the steel. At this time, the thickness of the slag layer of the molten steel is controlled to be 1 cm, the oxygen activity of the molten steel is controlled to be 25 ppm, and the temperature of the molten steel is controlled to be 1580°C;
[0069] (2) feeding the tellurium-containing cored wire directly into the ladle, the feeding position being above the bottom blowing argon hole, the wire feeding speed of the wire feeder being 2.5 m / s, and bottom blowing argon being performed during the wire feeding process, the argon flow rate of the argon bottom blowing being 320 NL / min;
[0070] (3) After all the tellurium-containing cored wires are fed, the resulting molten steel is post-treated by covering the surface of the molten steel with carbonized rice husks and performing bottom blowing of argon gas. The argon flow rate of the bottom blowing is 120 NL / min. After the argon blowing time is 13 minutes, the temperature is measured and sampled again. After the composition and temperature reach the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
[0071] In the on-site production of this comparative example, the feeding process is stable, the reaction is gentle, and there is no violent splashing.
[0072] The tellurium content of the tellurium-containing free-cutting steel prepared by the process of this embodiment is 32 ppm as measured by ICP. The tellurium recovery rate is calculated to be 57% based on the added amount.
[0073] Comparative Example 3:
[0074] This comparative example is basically the same as Example 3, except that:
[0075] This embodiment provides a tellurium-modified gear steel, whose main components (wt%) are: C: 0.19%, Si: 0.08%, Mn: 1.31%, P: 0.024%, S: 0.028%, Cr: 1.18%, Al: 0.039%, and the rest are Fe and unavoidable impurity elements. The smelting process adopted in this process is: electric furnace smelting → LF furnace refining → RH furnace refining → continuous casting, and a tellurium-containing cored wire with a total length of 50m is fed at the end of RH refining.
[0076] The tellurium-containing cored wire selected in this embodiment is composed of a cored tube and a core material. The cored tube is 08 steel with a thickness of 0.5 mm. The core material is pure tellurium powder. The weight of the core material per meter of the cored wire is 370 g. The outer diameter of the tellurium-containing cored wire is φ11 mm.
[0077] The process of feeding tellurium cored wire is:
[0078] (1) At the end of steel refining, after the adjustment of other components except tellurium is completed, tellurium-containing cored wire is fed into the steel. At this time, the thickness of the slag layer of the molten steel is controlled to be about 1 cm, the oxygen activity of the molten steel is 48 ppm, and the temperature of the molten steel is 1565°C;
[0079] (2) feeding the tellurium-containing cored wire directly into the wire feeder at one time, the wire feeding speed of the wire feeder is 1.5 m / s, and argon is blown bottom during the wire feeding process, and the argon flow rate of the argon bottom blowing is 280 NL / min;
[0080] (3) After feeding the tellurium-containing cored wire, argon is blown from the bottom at a flow rate of 140 NL / min for 12 minutes. The temperature is then measured and sampled again. When the composition and temperature reach the target steel liquid's finished product process requirements, the subsequent ladle tapping process is carried out.
[0081] In the on-site production of this comparative example, the feeding process is stable, the reaction is gentle, and there is no violent splashing.
[0082] The tellurium content of the tellurium-containing gear steel prepared by the process of this embodiment is 9 ppm as measured by ICP. The tellurium recovery rate is calculated to be 37% based on the added amount.
[0083] The actual tellurium yields of Comparative Examples 1, 2, and 3 were compared with those of Examples 1, 2, and 3. The results are shown in Table 1 below:
[0084] Table 1 Tellurium yield of sulfur-containing steel
[0085]
[0086] Comparative Examples 1, 2 and 3 did not perform tellurium modification according to the process provided by the present invention, and their actual yields were all lower than those in the embodiment. The present invention provides a process for improving tellurium modification of sulfur-containing steel, with a tellurium yield higher than 75%, and a relative error of less than 10%.
Claims
1. A method for producing tellurium-containing and sulfur-containing steel, the process flow of which is converter → LF furnace refining → VD / RH furnace refining → continuous casting, characterized in that: The chemical composition of the steel is as follows by weight: C=0.05-0.49%, Si=0.01-1.2%, Mn=0.60-1.60%, P≤0.025%, S=0.02-0.36%, V=0.08-1.20%, Cr≤0.3%, Mo≤0.08%, N=0.01-0.02%, Al≤0.02%, O≤0.0025%, Te=0.0001-0.008%, 0.075[S]≤Te≤0.0045%; The rest is Fe and unavoidable impurity elements; The key process steps include: 1) Molten steel refining: At the end of the molten steel refining, after the adjustment of other components except tellurium is completed, argon is blown at the bottom for full stirring for 3 to 5 minutes, and the argon flow rate of the bottom blowing argon is 150 to 300 NL / min, and then tellurium-containing cored wire is added to the molten steel for alloying, and the thickness of the molten steel slag layer is controlled to be about 1.2 to 1.5 cm at this time; 2) Tellurium feeding: Before feeding tellurium, the oxygen activity in the molten steel must be 5-40ppm. The specific oxygen activity needs to be further determined according to the target tellurium content of the steel grade. The target oxygen activity = (-0.3*target tellurium content + 27) ± 3, the unit of oxygen activity is ppm, and the unit of target tellurium content is ppm; the temperature of the molten steel is 40-45°C above the liquidus of the target production steel grade; the tellurium-containing cored wire is divided into several sections and fed into the ladle in sequence. The feeding position is above the bottom blowing argon hole, 20-30m is fed each time, the interval is 10-15s, the wire feeding speed of the wire feeding machine is 2-3m / s, no bottom blowing of argon is performed during the wire feeding process, and argon bottom blowing is performed during the interval between two feedings. The argon flow rate of the argon bottom blowing is 120-250NL / min; 3) Argon blowing: Bottom blowing of argon during molten steel refining can be divided into three stages: Stage 1: fine-tuning of other components except tellurium, at which time the argon flow rate of bottom blowing argon is always 150-300NL / min; Stage 2: feeding tellurium-containing cored wire, no argon bottom blowing during the feeding process, argon bottom blowing during the feeding interval, the argon flow rate of the bottom blowing argon is 120-250NL / min; Stage 3: after feeding the tellurium-containing wire, continue to blow argon at the bottom, at which time the argon flow rate of the bottom blowing argon is 100-180NL / min, and the blowing time is 10-15min; 4) Post-processing: Optimize the post-feeding wire protection process. After feeding all tellurium-containing cored wires, post-process the obtained molten steel. Cover the surface of the molten steel with carbonized rice husks and perform bottom blowing of argon. The argon flow rate of the bottom blowing is 100-180NL / min. After the argon blowing time is 10-15min, the temperature is measured and sampled again. After the composition and temperature meet the finished product process requirements of the target molten steel, the subsequent ladle tapping process is carried out.
2. The method for producing tellurium-containing and sulfur-containing steel according to claim 1, characterized in that The step 2) feeding tellurium: the core tube and core material of the tellurium-containing cored wire are composed of: the core material is a mixed component of pure tellurium powder and industrial pure iron powder, the ratio of pure tellurium powder to industrial pure iron powder is 1: (1.5-2.5), the weight of the core material per meter of the cored wire is 330-360g, and the outer diameter of the tellurium-containing cored wire is φ10-13mm; the core tube is low-carbon steel with a thickness of 0.3-0.4mm.
3. The method for producing tellurium-containing and sulfur-containing steel according to claim 1 is characterized in that In the step 2) of feeding tellurium, the wire feeding machine guide tube should be vertically inserted into the molten steel, and the outlet of the wire feeding machine guide tube should be 20 to 40 cm away from the molten steel surface.
4. The method for producing tellurium-containing and sulfur-containing steel according to claim 1, characterized in that: The sulfur-containing tellurium-containing steel is a non-quenched and tempered steel, and its composition is C=0.37%, Si=0.65%, Mn=1.00%, P=0.025%, S=0.035%, Cr=0.16%, V=0.29%, Al=0.006%, N=0.017%, O≤0.0025%, Te=0.0001-0.008% by mass percentage, and the rest are Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the molten steel temperature needs to be controlled at 1531-1536°C.
5. The method for producing tellurium-containing and sulfur-containing steel according to claim 1, characterized in that: The sulfur-containing tellurium-containing steel is a free-cutting steel, and its chemical composition is C=0.063%, Si=0.009%, Mn=1.266%, P=0.025%, S=0.05%, Al=0.001%, O≤0.0025%, Te=0.0001-0.008% by mass percentage, and the rest are Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the molten steel temperature needs to be controlled at 1554-1559°C.
6. The method for producing tellurium-containing and sulfur-containing steel according to claim 1, characterized in that: The sulfur-containing tellurium-containing steel is a gear steel, and its composition by mass percentage is C=0.19%, Si: 0.08%, Mn=1.3%, P: 0.022%, S=0.028%, Cr=1.18%, Al=0.039%, O≤0.0025%, Te=0.0001-0.008%, and the rest is Fe and unavoidable impurity elements. Before feeding the tellurium-containing cored wire, the oxygen activity is 10-20ppm, and the molten steel temperature needs to be controlled at 1533-1538°C.