Method for designing components of high-flux high-entropy alloy

The gradient transition zone of high-entropy alloy is formed through a directional solidification furnace and induction infusion system, which solves the problem of low screening efficiency of high-entropy alloy components, and realizes high-precision and efficient component design, which is suitable for industrial applications.

CN118932202AActive Publication Date: 2024-11-12AVIC BEIJING INST OF AERONAUTICAL MATERIALS

Patent Information

Application Number
CN202411151211.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

The existing high-entropy alloy components have low screening efficiency, high equipment costs, complex operation, small sizes of the sample prepared and do not have excellent performance in industrial applications.

Method used

Using a directional solidification furnace and induction infusion system, a gradient transition zone is formed by forming a melt between the initial sample and the master alloy ingot to prepare high-throughput high-entropy alloy samples to achieve uniform linear components and high-precision screening.

Benefits of technology

It improves the accuracy and performance data reliability of high-entropy alloy composition design, reduces equipment costs, simplifies the operation process, and realizes high-throughput high-entropy alloy samples with large size and excellent performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides a method for designing components of a high-flux high-entropy alloy. The method comprises the following steps: S1) preparing an initial sample of pure metal or alloy; s2) preparing a master alloy ingot according to the components of the high-entropy alloy; s3) assembling the initial sample at the bottom of a shell, and fixing the shell on a pulling device of a directional solidification furnace, so that one part of the initial sample is exposed out of the liquid level of a cooling tank, and the other part of the initial sample is immersed in the cooling liquid of the cooling tank; s4) assembling the master alloy ingot at the upper part of an induction instillation system of the directional solidification furnace, and starting a heating power supply of the directional solidification furnace; and S5) starting the induction instillation system until the master alloy ingot is molten and instilled into the shell, and cooling and solidifying after heat preservation. The components of the high-throughput sample prepared by the method provided by the invention are uniform and linear, and the component screening precision is higher; the method can be used for efficiently preparing a single-element or multi-element coupling change high-throughput sample, the reliability of obtained performance data is higher, and the industrial application potential of the alloy is higher.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high entropy alloys, and in particular to a method for designing high-flux high entropy alloy components. Background Art

[0002] High entropy alloy is a disruptive new alloy system developed in recent years. It is composed of 5 or more main elements, each of which is mixed in an equiatomic ratio or a nearly equiatomic ratio, and the atomic percentage of each main element is between 5% and 35%. Therefore, it is also called multi-principal element, equiatomic ratio or nearly equiatomic ratio alloy. Compared with traditional alloys, high entropy alloys have a high entropy effect in thermodynamics, a slow diffusion effect in kinetics, a lattice distortion effect in structure, and a cocktail effect in performance. Under the coupling of multiple mechanisms, high entropy alloys have many excellent properties that traditional materials cannot match, and are therefore regarded as one of the key materials that are expected to solve the bottleneck problem of material performance in the current engineering field.

[0003] With the further development of research in the field of high entropy alloys, the definition of high entropy alloys has been expanded, and the efficient composition design and preparation methods of high entropy alloys have become the key to their industrial application. The composition design and efficient preparation methods commonly used for high entropy alloy composition screening include discrete template coating method, multi-target co-sputtering method and laser melting deposition method, but these methods generally have the following problems: First, the equipment cost is high, the control parameters are numerous, and the operation process is complicated; second, the prepared samples can only be pre-designed independent composition points, and it is impossible to prepare samples with linear composition changes, resulting in inaccurate composition screening; third, the size of the prepared samples is generally small, and the mechanical properties of the alloy can only be evaluated through compression tests. The obtained alloy composition may not have the optimal performance after industrial production.

[0004] The above problems limit the screening efficiency of high entropy alloy components. Therefore, it is urgent to develop low-cost, high-precision composition design and efficient preparation methods that can prepare large-scale high entropy alloy samples. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a method for high-throughput high-entropy alloy composition design. The method provided in this application can design different high-entropy alloy compositions at the same time with higher accuracy and higher reliability of performance data.

[0006] In view of this, the present application provides a method for high-throughput high-entropy alloy composition design, comprising the following steps: S1) preparing an initial sample of pure metal or alloy; the elements of the pure metal or alloy are selected from one or two of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; S2) preparing raw materials according to the high entropy alloy composition, and then preparing a master alloy ingot; the master alloy ingot is prepared from at least three elements of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; S3) assembling the initial sample at the bottom of the mold shell, fixing the mold shell on the pulling device of the directional solidification furnace, and adjusting the position of the mold shell so that a part of the initial sample is exposed above the liquid surface of the cooling tank, and the rest of the initial sample is immersed in the coolant of the cooling tank; the initial samples in the mold shell can be samples of the same type or samples of different types; S4) assembling the master alloy ingot on the upper part of the induction dripping system of the directional solidification furnace, turning on the heating power of the directional solidification furnace to make the temperature higher than the melting point of the initial sample and the melting point of the master alloy ingot; S5) turning on the induction dripping system until the master alloy ingot is melted and dripped into the mold shell, keeping the temperature to form a gradient transition zone between the initial sample and the melt of the master alloy ingot, and then cooling and solidifying.

[0007] Preferably, the mold shell is a ceramic mold shell, and the ceramic mold shell is prepared by an investment casting method.

[0008] Preferably, the height of the initial sample exposed from the liquid surface of the cooling tank is 1 / 4 to 1 / 2 of the initial sample, and the coolant is a gallium indium tin alloy.

[0009] Preferably, the directional solidification furnace is kept in a vacuum or an inert gas is introduced, and the vacuum is 3×10 -3 ~9×10 -1 Pa.

[0010] Preferably, the temperature of the directional solidification furnace is 50-100° C. above the melting point of the initial sample and the melting point of the master alloy ingot.

[0011] Preferably, in step S4), the heating rate of the directional solidification furnace is 10-15°C / min, and the holding time after reaching the temperature is 20-40min.

[0012] Preferably, in step S5), the power of the induction coil of the induction dripping system is 30-40 kW, the rotation speed of the master alloy ingot is 5-10 rad / min, the feed rate is 0.3-0.5 mm / s, and the insulation time is 0-30 min.

[0013] Preferably, the cooling and solidification specifically comprises: The pulling device is turned on at a moving speed of 0.001~20mm / s, and the shell moves vertically from top to bottom into the cooling tank; Or turn off the heating power of the directional solidification furnace to allow the alloy melt inside the shell to cool and solidify naturally.

[0014] Preferably, step S5) further includes: The solidified high entropy alloy sample is taken out and then subjected to stress relief annealing; The high entropy alloy samples after stress relief annealing were sectioned longitudinally, and the composition, microstructure and mechanical properties of the bonding area were analyzed to screen out high entropy alloy components with excellent performance.

[0015] Preferably, the stress relief annealing is performed at a temperature of 300-900° C. for 1-4 hours.

[0016] The present application provides a method for designing a high-throughput high-entropy alloy composition, which first prepares an initial sample of a pure metal or alloy, then prepares a master alloy ingot according to the high-entropy alloy composition, and then assembles the initial sample at the bottom of the shell, and finally melts the initial sample and the master alloy ingot by heating in a directional solidification furnace, and the melt of the initial sample and the master alloy ingot forms a gradient transition zone, and after cooling and solidification, a high-throughput high-entropy alloy with a designed composition is obtained. The method for designing a high-throughput high-entropy alloy composition provided by the present application designs an initial sample, and drips the melt of the high-entropy master alloy ingot onto the surface of the molten initial sample, thereby forming a gradient transition zone, making the high-entropy alloy composition uniform and linear, and the screening accuracy is higher, realizing the efficient preparation of high-throughput high-entropy alloy samples with single-element or multi-element coupled changes, and the obtained performance data has higher reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic diagram of the mold shell of the present invention and a top view of the actual object; Figure 2 A schematic diagram of the equipment and mold shell position for preparing high-throughput high-entropy alloy samples of the present invention; Figure 3 A schematic diagram of the process of preparing a high-throughput high-entropy alloy sample according to the present invention; Figure 4 This is a photo of a cylindrical high-flux high-entropy alloy sample prepared in Example 1 of the present invention; Figure 5 A microstructure photograph of the bonding area of ​​a high entropy alloy cylindrical sample having a coupled linear gradient change zone of Ti and Al elements prepared in Example 2 of the present invention after sectioning; Figure 6 This is an element line scanning spectrum of the bonding area of ​​a high entropy alloy cylindrical sample having a Ti and Al element coupled linear gradient change zone prepared in Example 2 of the present invention after being cut. DETAILED DESCRIPTION

[0018] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0019] In view of the problem of low efficiency in screening high-entropy alloy components in the prior art, the present application provides a method for designing high-throughput high-entropy alloy components, which uses a single-element or multi-element coupled sample as a basic sample, combined with a high-entropy alloy master alloy ingot, to form a high-entropy alloy sample with a gradient transition, and finally performs performance screening to obtain accurate customization of the high-entropy alloy composition. Furthermore, the initial sample may not be limited to one sample, so that the composition design of high-throughput high-entropy alloys can be achieved. Specifically, an embodiment of the present invention discloses a method for designing high-throughput high-entropy alloy components, comprising the following steps: S1) preparing an initial sample of pure metal or alloy; the elements of the pure metal or alloy are selected from one or two of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; S2) except for the elements in step S1), preparing raw materials according to the high entropy alloy composition, and then preparing a master alloy ingot; the master alloy ingot is prepared from at least three elements of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; S3) assembling the initial sample at the bottom of the mold shell, fixing the mold shell on the pulling device of the directional solidification furnace, and adjusting the position of the mold shell so that a part of the initial sample is exposed from the liquid surface of the cooling tank, and the rest of the initial sample is placed in the cooling tank; the initial samples in the mold shell can be samples of the same type or samples of different types; S4) assembling the master alloy ingot on the upper part of the induction dripping system of the directional solidification furnace, turning on the heating power of the directional solidification furnace to make the temperature higher than the melting point of the initial sample and the melting point of the master alloy ingot; S5) turning on the induction dripping system until the master alloy ingot is melted and dripped into the mold shell, keeping the temperature to form a gradient transition zone between the initial sample and the melt of the master alloy ingot, and then cooling and solidifying.

[0020] In the method for designing high-throughput high-entropy alloy compositions provided in the present application, in step S1), an initial sample of pure metal or alloy is first prepared, wherein the element of the pure metal or alloy is selected from one or two of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; that is, the initial sample of the above-mentioned pure metal can be prepared alone, or the initial sample of the above-mentioned two elements can be prepared, and the element ratio of the initial sample of the two elements can be prepared according to demand; in a specific embodiment, pure metal Fe rods, pure metal Co rods, pure metal Ni rods, pure metal Al rods, and pure metal Ti rods are prepared; or NiTi intermediate alloy rods, TiAl intermediate alloy rods, or NiCr50 intermediate alloy rods are prepared. The preparation of the rods of the initial alloy is prepared according to the conventional technical means of those skilled in the art, and can be prepared by casting, forging, powder metallurgy, or additive manufacturing. The melting point of the initial sample is T A .

[0021] In step S2), raw materials are prepared according to the high entropy alloy composition to prepare a master alloy ingot; the high entropy alloy composition is selected from at least three elements of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B, that is, three or more of the above elements are selected as needed to prepare the high entropy alloy composition; for example, the master alloy ingot is a high entropy alloy master alloy ingot of FeCoNiAl with an equiatomic ratio or a high entropy alloy master alloy ingot of (FeCoNiCr) with a specific atomic ratio. 96 Al2Ti2 high entropy alloy master alloy ingot; the master alloy ingot can be obtained by melting and pouring in a vacuum consumable melting furnace, or the master alloy ingot can be obtained by melting and pouring in a vacuum induction melting furnace. The melting point of the master alloy ingot is T B .

[0022] In step S3), the initial sample is assembled at the bottom of the mold shell; in this step, the mold shell is a mold shell with a structure familiar to those skilled in the art, and this application does not impose any particular limitation on this. Preferably, the mold shell is a ceramic mold shell. The placement structure of the initial sample in the mold shell is as follows: Figure 1As shown, in the left figure, 1 is the gate, 2 is the main body of the rod-shaped sample mold shell, 3 is the initial sample preset in the mold shell, and 4 is the base; the right figure is a top view of the initial sample in the mold shell; in this example mold shell, three initial samples are preset, and the initial samples are only preset at the bottom of the mold shell, and the upper part is the original rod-shaped mold shell for dripping the high entropy alloy melt. In the present application, the initial samples preset in the mold shell can be the same samples or different samples. Among the different sample selections, single-element samples or two-element coupled samples can be selected. For example, the bottom of the mold shell can be simultaneously equipped with five pure metal bars, namely pure metal Fe bars, pure metal Co bars, pure metal Ni bars, pure metal Al bars and pure metal Ti bars; or it can be equipped with three intermediate alloy bars, namely NiTi intermediate alloy bars, TiAl intermediate alloy bars and NiCr50 intermediate alloy bars, or a combination of pure metal bars and intermediate alloy bars of pure metal Fe bars, pure metal Co bars, NiTi intermediate alloy bars and TiAl intermediate alloy bars.

[0023] After the shell is prepared, it is fixed on the pulling device of the directional solidification furnace. The position of the shell is adjusted by the pulling device so that a part of the initial sample is exposed to the liquid surface of the cooling tank, and the rest is immersed in the coolant of the cooling tank; the directional solidification furnace is a directional solidification furnace for preparing high entropy alloys well known to those skilled in the art, which includes a stretching device, a heating device, an induction dripping system, a cooling tank, etc. The specific setting position is well known to those skilled in the art, and this application does not impose any special restrictions on this. The height of the initial sample exposed to the liquid surface of the cooling tank is 1 / 4 to 1 / 2 of the initial sample, more specifically 1 / 4, 1 / 3 or 1 / 2; the coolant can be specifically selected from gallium indium tin alloy.

[0024] In step S4), the master alloy ingot is mounted on the upper part of the induction dripping system of the directional solidification furnace, as follows: Figure 2 As shown, Figure 2 5 is a high entropy alloy master alloy ingot, 11 is an induction coil, 12 is an upper cover plate, 13 is a heating body, 14 is a furnace body, 15 is a cooling tank, 16 is a gallium indium tin coolant, and 17 is a stretching rod. Then, the vacuum pump of the directional solidification furnace is turned on to make the vacuum degree in the equipment reach 3×10 -3 ~9×10 -1 Pa, maintain vacuum or pass inert gas for protection; turn on the heating power of the directional solidification furnace to make the temperature higher than the melting point of the initial sample and the melting point of the master alloy ingot; specifically, the temperature of the directional solidification furnace is the melting point T of the initial sample A and the melting point T of the master alloy ingot BThe temperature is above 50-100°C, the heating rate of the directional solidification furnace is 10-15°C / min, and the holding time after reaching the temperature is 20-40min; to ensure that the shell is fully preheated and the portion of the bottom initial sample exposed from the cooling tank is melted.

[0025] In step S5), the induction dripping system is turned on to melt the high entropy alloy and drip it into the shell mold to contact the initial sample melted in the shell mold; the power of the induction coil in the induction dripping system is 30~40kW, the rotation speed of the master alloy ingot is 5~10rad / min, and the feed rate is 0.3~0.5mm / s. Specifically, the power of the induction coil in the induction dripping system is 35~40kW, the rotation speed of the master alloy ingot is 6~8rad / min, and the feed rate is 0.3~0.4mm / s. The induction dripping system is kept warm after the dripping is completed to allow the melt in the bonding area of ​​the initial sample and the high entropy alloy to mix and diffuse to form a gradient transition zone. Finally, cooling and solidification are performed to achieve the design of the high-flux high-entropy alloy composition in the linear gradient change zone. The cooling and solidification are specifically as follows: The pulling device is turned on at a moving speed of 0.001~20mm / s, and the mold shell moves vertically from top to bottom into the cooling tank to solidify the molten alloy inside the mold shell; or the heating power of the directional solidification furnace is turned off to allow the molten alloy inside the mold shell to cool and solidify naturally.

[0026] The schematic diagram of the process flow of the high-throughput high-entropy alloy composition design in the present application is as follows: Figure 3 As shown, 6 is the liquid zone formed by dripping the high entropy alloy into the shell after induction melting; this process is specifically as follows: first assemble the initial sample, then assemble the high entropy alloy master alloy ingot, drip the high entropy alloy melt, then the high entropy alloy melt and the initial sample melt form a liquid zone, and finally form an element diffusion zone.

[0027] After preparing the above-mentioned high-throughput high-entropy alloy sample, the present application further includes a screening process, specifically: The solidified high entropy alloy sample is taken out and then subjected to stress relief annealing; The high entropy alloy samples after stress relief annealing were sectioned longitudinally, and the composition, microstructure and mechanical properties of the bonding area were analyzed to screen out high entropy alloy components with excellent performance.

[0028] In the above process, the stress relief annealing temperature is 300~900℃, and the temperature is kept for 1~4h; the composition of the bonding area is tested by electron probe, the tissue morphology is tested by metallographic microscope, scanning electron microscope, and transmission electron microscope, the mechanical properties mainly include microhardness, and tensile properties test is carried out.

[0029] The method for high-throughput high-entropy alloy composition design provided in the present application is particularly suitable for preparing high-entropy alloy samples with coupled changes of one or two elements, and more specifically includes the following steps: 1. Raw materials and shell preparation: (1) According to the type and ratio of one or two elements to be studied, pure metal or alloy bars or plates are prepared by casting, forging, powder metallurgy or additive manufacturing, or a combination of these methods, with a melting point of T A ; The pure metal or alloy bar or plate is composed of one or two elements selected from Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; (2) Prepare the raw materials according to the high entropy alloy composition, use a vacuum consumable melting furnace or a vacuum induction melting furnace to melt and cast into a master alloy ingot, the melting point of which is T B ; The high entropy alloy master alloy ingot is composed of at least three elements of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; (3) Using investment casting method to prepare rod-shaped or plate-shaped ceramic shell; 2. Preparation and composition screening of high entropy alloy samples: Efficient preparation of high entropy alloys with linear gradient change zones using a modified Bridgeman directional solidification apparatus (1) Assemble the rod or plate of pure metal or alloy at the bottom of the ceramic shell, and fix it as a whole on the stretching rod of the directional solidification furnace. According to the needs, different types of pure metal or alloy rods can be assembled in the same shell at the same time to realize the preparation of single element or two elements coupled high-throughput samples; adjust the height of the stretching rod so that 1 / 4~1 / 2 of the pure metal or alloy rod or plate is exposed above the liquid surface of the cooling tank, and the rest is completely immersed in the cooling tank. The coolant in the cooling tank is gallium indium tin alloy; (2) Assembling a high entropy alloy master alloy ingot on the upper part of the induction dripping coil of the directional solidification furnace; (3) Turn on the vacuum pump of the directional solidification furnace to make the vacuum degree in the equipment reach 3×10 -3 ~9×10 -1 Pa, maintain vacuum or pass inert gas for protection; (4) Set the furnace temperature to T A and T BWhen the temperature is 50-100℃ above the higher temperature, turn on the power of the directional solidification furnace to heat up the upper and lower heating bodies in the furnace at a heating rate of 10-15℃ / min. Keep the temperature for 20-40min after reaching the temperature to ensure that the ceramic shell is fully preheated. At the same time, the pure metal or alloy rod or plate at the bottom of the shell that is exposed to the cooling tank is melted; (5) Turn on the induction dripping system, adjust the induction coil power to 30-35 kW, the rotation speed of the high entropy alloy ingot to 8-10 rad / min, and the feed rate to 0.3-0.4 mm / s, and then turn off the induction dripping system after a sufficient amount of high entropy alloy is melted; (6) After the high entropy alloy is dripped, the temperature is kept at 0-30 min to allow the melt in the bonding area of ​​the pure metal or alloy and the high entropy alloy to mix and diffuse, forming a gradient transition zone; (7) The pulling device is turned on at a moving speed of 0.001-20 mm / s, and the ceramic shell moves vertically from top to bottom into the cooling tank to solidify the alloy melt inside the shell; or the heating power of the directional solidification furnace is turned off to allow the alloy melt inside the shell to cool and solidify naturally, thereby completing the efficient preparation of a high entropy alloy sample with a linear gradient change zone; 3. Ingredient screening: (1) After the temperature in the furnace is naturally cooled to room temperature, the high entropy alloy sample is taken out of the directional solidification furnace, and the mold shell is removed by sand blowing or machining to obtain a high entropy alloy sample; (2) Place the high entropy alloy sample in a box-type resistance furnace and keep it at 300~900℃ for 1~4h to remove residual stress; (3) The high-entropy alloy sample is cut longitudinally, and the distribution and changes of the components in the bonding area are tested using an electron probe. The microstructure of the bonding area between the pure metal or alloy and the high-entropy alloy is observed using a metallographic microscope, a scanning electron microscope, and a transmission electron microscope. The room temperature and high temperature microhardness of the bonding area is tested, and a tensile property test is performed, so as to accurately screen out high-entropy alloy components with excellent performance.

[0030] The present application provides a method for designing the composition of a high-throughput high-entropy alloy. The composition of the prepared high-throughput high-entropy alloy sample is uniform and linear, and the composition screening accuracy is higher; single-element or multi-element coupled change high-throughput samples can be efficiently prepared; large-scale high-throughput samples can be prepared, the obtained performance data is more reliable, and the alloy has greater potential for industrial application; the equipment cost is significantly reduced, and the control parameters are greatly reduced, simplifying the operation process.

[0031] In order to further understand the present invention, the preparation method of the high-flux high-entropy alloy provided by the present invention is described in detail below in combination with examples, and the protection scope of the present invention is not limited by the following examples.

[0032] Example 1 The preparation of a high entropy alloy sample with a nominal composition of FeCoNiAl as the main body and a gradient transition zone of Fe, Co, Ni, Al, and Ti elements, with a sample size of Φ15mm×120mm, is achieved by the following steps: 1. Raw materials and shell preparation: (1) Pure metal Fe, Co, Ni, Al, and Ti bars are used, and their melting points are 1538°C, 1495°C, 1455°C, 660°C, and 1668°C, respectively. The surface of the bars is processed to a roughness of Ra = 3.2 μm, and the size is Φ14.5 mm × 60 mm; (2) The raw materials of FeCoNiAl high entropy alloy are prepared according to equiatomic ratios, with the corresponding weight percentages being: Fe 27.8%; Co 29.4%; Ni 29.3%; and Al 13.5%. The alloy is melted twice in a vacuum induction melting furnace to ensure the uniformity of the composition and cast into a high entropy alloy master alloy ingot, the melting point of which is about 1580°C. (3) The ceramic shell of the rod-shaped specimen is prepared by investment casting; 2. Preparation and composition screening of high entropy alloy samples: Efficient preparation of high entropy alloys with linear gradient change zones of Fe, Co, Ni, Al, and Ti using a modified Bridgeman directional solidification device (1) Assemble pure metal Fe, Co, Ni, Al, and Ti rods at the bottom of the ceramic shell (the specific structural diagram is shown in Figure 1 As shown in the figure), fix it as a whole on the stretching rod of the directional solidification furnace; adjust the height of the stretching rod so that 1 / 2 of the pure metal rod is exposed above the liquid surface of the cooling tank, and the rest is completely immersed in the cooling tank. The coolant in the cooling tank is gallium indium tin alloy (the specific structural schematic diagram is shown in the figure). Figure 2 shown); (2) Assemble the FeCoNiAl high entropy alloy master alloy ingot on the upper part of the induction dripping coil of the directional solidification furnace (the specific structural schematic diagram is shown in Figure 2 shown); (3) Turn on the vacuum pump of the directional solidification furnace to make the vacuum degree in the equipment reach 10 -1 Pa; (4) Set the furnace temperature to 1720°C, turn on the heating power of the directional solidification furnace to heat up the upper and lower heating bodies in the furnace at a heating rate of 15°C / min, and keep the temperature for 30 minutes after reaching the temperature to ensure that the ceramic shell is fully preheated. At the same time, the part of the pure metal rod at the bottom of the shell that is exposed to the cooling tank is melted; (5) Turn on the induction dripping system, adjust the induction coil power to 30 kW, the rotation speed of the FeCoNiAl high entropy alloy master alloy ingot to 8 rad / min, and the feed rate to 0.3 mm / s, and then turn off the induction dripping system after a sufficient amount of high entropy alloy is melted; (6) After the high entropy alloy is dripped, the temperature is kept for 20 minutes to allow the melt in the bonding area of ​​the pure metal and the high entropy alloy to mix and diffuse, forming a gradient transition zone; (7) The pulling device is turned on at a moving speed of 0.2 mm / s, and the ceramic shell moves vertically from top to bottom into the cooling tank, so that the alloy melt inside the shell solidifies, thereby completing the efficient preparation of a high-entropy alloy sample with a linear gradient change zone of Fe, Co, Ni, Al, and Ti.

[0033] 3. Ingredient screening: (1) After the temperature in the furnace is naturally cooled to room temperature, the cooled high entropy alloy sample is taken out of the directional solidification furnace, and the shell is removed by sand blowing or machining to obtain a high entropy alloy sample (specific sample is as follows: Figure 4 shown); (2) Place the high entropy alloy sample in a box-type resistance furnace and keep it at 400°C for 2 h to remove residual stress; (3) The high-entropy alloy sample is cut longitudinally, and the distribution and changes of the components in the bonding area are tested using an electron probe. The microstructure of the bonding area between the pure metal or alloy and the high-entropy alloy is observed using a metallographic microscope, a scanning electron microscope, and a transmission electron microscope. The room temperature and high temperature microhardness of the bonding area is tested, and a tensile property test is performed, so as to accurately screen out high-entropy alloy components with excellent performance.

[0034] Example 2 The nominal composition is (FeCoNiCr) 96 The preparation of a high entropy alloy sample with Al2Ti2 as the main body and a gradient transition zone with coupling of Ni and Ti elements, coupling of Ti and Al elements, and coupling of Ni and Cr elements, with a sample size of Φ15mm×120mm, is achieved by the following steps: 1. Raw materials and shell preparation: (1) NiTi, TiAl, and NiCr50 master alloy bars are used, with melting points of approximately 1310°C, 1460°C, and 1290°C, respectively. The surface of the bars is processed to a roughness of Ra = 3.2 μm and a size of Φ14.5 mm × 60 mm; (2) According to (FeCoNiCr) 96 The raw materials of Al2Ti2 high entropy alloy are prepared with the corresponding weight percentages of Fe 24.1%, Co 25.4%, Ni 25.3%, Cr 22.5%, Al 1.0%, and Ti 1.7%. The alloy is melted twice in a vacuum induction melting furnace to ensure the uniformity of the composition and cast into a master alloy ingot, with a melting point of about 1680°C. (3) The ceramic shell of the rod-shaped specimen is prepared by investment casting; 2. Preparation and composition screening of high entropy alloy samples: The improved Bridgeman directional solidification equipment is used to efficiently prepare high entropy alloys with Ni, Ti, Ti, Al, and Ni, Cr coupled linear gradient change zones. (1) NiTi, TiAl, and NiCr50 master alloy rods are assembled at the bottom of the ceramic shell, and the whole is fixed on the stretching rod of the directional solidification furnace; the height of the stretching rod is adjusted so that 1 / 3 of the pure metal rod is exposed above the liquid surface of the cooling tank, and the rest is completely immersed in the cooling tank. The coolant in the cooling tank is gallium indium tin alloy (the specific structural diagram is shown in the figure). Figure 2 shown); (2) (FeCoNiCr) 96 The Al2Ti2 high entropy alloy master alloy ingot is assembled on the upper part of the induction dripping coil of the directional solidification furnace (the specific structural diagram is shown in Figure 2 shown); (3) Turn on the vacuum pump of the directional solidification furnace to make the vacuum degree in the equipment reach 10 -1 Pa; (4) Set the furnace temperature to 1720°C, turn on the heating power of the directional solidification furnace to heat up the upper and lower heating bodies in the furnace at a heating rate of 15°C / min, and keep the temperature for 25 minutes after reaching the temperature to ensure that the ceramic shell is fully preheated. At the same time, the part of the intermediate alloy rod at the bottom of the shell that is exposed to the cooling tank is melted; (5) Turn on the induction drip system and adjust the induction coil power to 35kW, (FeCoNiCr) 96 The Al2Ti2 high entropy alloy master alloy ingot rotates at a speed of 10 rad / min and a feed rate of 0.4 mm / s until a sufficient amount of high entropy alloy is melted and then the induction drip system is turned off; (6) After the high entropy alloy is dripped, the temperature is kept for 30 minutes to allow the melt in the intermediate alloy and high entropy alloy bonding area to mix and diffuse, forming an element coupling gradient transition zone; (7) Turn off the heating power of the directional solidification furnace to allow the alloy melt inside the shell to cool and solidify naturally, thereby completing the efficient preparation of a high entropy alloy having coupled linear gradient change zones of Ni, Ti, Ti, Al, and Ni, Cr elements.

[0035] 3. Ingredient screening: (1) After the temperature in the furnace is naturally cooled to room temperature, the cooled high entropy alloy sample is taken out of the directional solidification furnace, and the shell is removed by sand blowing or machining to obtain a high entropy alloy sample; (2) The high entropy alloy sample was placed in a box-type resistance furnace and kept at 650 °C for 4 h to remove residual stress; (3) The high-entropy alloy sample is cut longitudinally, and the distribution and changes of the components in the bonding area are tested using an electron probe. The microstructure of the bonding area between the pure metal or alloy and the high-entropy alloy is observed using a metallographic microscope, a scanning electron microscope, and a transmission electron microscope. The room temperature and high temperature microhardness of the bonding area is tested, and a tensile property test is performed, so as to accurately screen out high-entropy alloy components with excellent performance.

[0036] like Figure 5 As shown, Figure 5 This is a microstructure photograph of the bonding area of ​​a high entropy alloy cylindrical sample with a linear gradient change zone of Ti and Al elements prepared in this embodiment after sectioning. Figure 5 It can be seen that the tissue in the combined area changes uniformly in gradient.

[0037] like Figure 6 As shown, Figure 6 This is the element line scanning spectrum of the bonding area of ​​the high entropy alloy cylindrical sample with Ti and Al element coupled linear gradient change zone prepared in this embodiment after cutting, right Figure 6 It can be seen that the elements in the combined area change with uniform gradient.

[0038] The above embodiments are only used to help understand the method and core idea of ​​the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

[0039] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for high-throughput high-entropy alloy composition design, comprising the following steps: S1) preparing an initial sample of pure metal or alloy; the elements of the pure metal or alloy are selected from one or two of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; S2) preparing raw materials according to the high entropy alloy composition, and then preparing a master alloy ingot; the master alloy ingot is prepared from at least three elements of Fe, Co, Ni, Al, Ti, Cu, Si, Ta, Nb, Cr, Zr, V, Mo, Hf, C, and B; S3) assembling the initial sample at the bottom of the mold shell, fixing the mold shell on the pulling device of the directional solidification furnace, and adjusting the position of the mold shell so that a part of the initial sample is exposed above the liquid surface of the cooling tank, and the rest of the initial sample is immersed in the coolant of the cooling tank; the initial samples in the mold shell can be samples of the same type or samples of different types; S4) assembling the master alloy ingot on the upper part of the induction dripping system of the directional solidification furnace, turning on the heating power of the directional solidification furnace to make the temperature higher than the melting point of the initial sample and the melting point of the master alloy ingot; S5) turning on the induction dripping system until the master alloy ingot is melted and dripped into the mold shell, keeping the temperature to form a gradient transition zone between the initial sample and the melt of the master alloy ingot, and then cooling and solidifying.

2. The method according to claim 1, characterized in that The mold shell is a ceramic mold shell, and the ceramic mold shell is prepared by an investment precision casting method.

3. The method according to claim 1, characterized in that The height of the initial sample exposed from the liquid surface of the cooling tank is 1 / 4 to 1 / 2 of the initial sample, and the coolant is a gallium indium tin alloy.

4. The method according to claim 1, characterized in that: The directional solidification furnace is kept in a vacuum or an inert gas is introduced, and the vacuum is 3×10 -3 ~9×10 -1 Pa.

5. The method according to claim 1, characterized in that The temperature of the directional solidification furnace is 50-100° C. above the melting point of the initial sample and the melting point of the master alloy ingot.

6. The method according to claim 1, characterized in that In step S4), the heating rate of the directional solidification furnace is 10-15°C / min, and the holding time after reaching the temperature is 20-40min.

7. The method according to claim 1, characterized in that In step S5), the power of the induction coil of the induction dripping system is 30-40 kW, the rotation speed of the master alloy ingot is 5-10 rad / min, the feed rate is 0.3-0.5 mm / s, and the insulation time is 0-30 min.

8. The method according to claim 1, characterized in that The cooling and solidification specifically includes: The pulling device is turned on at a moving speed of 0.001~20mm / s, and the shell moves vertically from top to bottom into the cooling tank; Or turn off the heating power of the directional solidification furnace to allow the alloy melt inside the shell to cool and solidify naturally.

9. The method according to any one of claims 1 to 8, characterized in that Step S5) further includes: The solidified high entropy alloy sample is taken out and then subjected to stress relief annealing; The high entropy alloy samples after stress relief annealing were sectioned longitudinally, and the composition, microstructure and mechanical properties of the bonding area were analyzed to screen out high entropy alloy components with excellent performance.

10. The method according to claim 9, characterized in that The stress relief annealing temperature is 300-900° C. and the temperature is kept for 1-4 hours.

Citation Information

Patent Citations

  • Directional solidification device for preparing TiAl radicle alloy bloom

    CN101112716A

  • Multifunctional melting and casting equipment applied to high-melting point and high-activity metal material

    CN106756073A

  • Ta-W-Nb-Al-Cr-Ti-Si series high-entropy alloy diffusion coating for high-throughput screening and preparation method of Ta-W-Nb-Al-Cr-Ti-Si series high-entropy alloy diffusion coating

    CN111876645A

  • High-throughput preparation method for metal parts

    CN113305283A

  • Cold crucible induction melting method for multi-element, high-activity and refractory high-entropy alloy

    CN115558814A

Cited By

  • High-entropy target body for deuterium-deuterium neutron generator, high-entropy target and preparation method of high-entropy target body

    CN119835853A