High-performance heat-resistant aluminum alloy stranded wire and preparation method thereof
Through a specific process, high-performance heat-resistant aluminum alloy stranded wires were prepared, which solved the problems of insufficient strength and high resistivity of existing aluminum alloy strands at high temperatures, and achieved high tensile strength, conductivity and resistance The thermal performance is improved to meet the high performance requirements of large-span wires.
Patent Information
- Application Number
- CN202411017735.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing high-strength heat-resistant aluminum alloy stranded wires have insufficient strength and safety performance and high resistivity at high temperatures, resulting in a lot of line losses and are difficult to meet the high performance needs of large-span wires.
Aluminum alloy materials with specific composition ratios are used for melting, borate, refining, casting, rolling, drawing, aging and annealing treatment, and high performance resistance with high tensile strength, high conductivity and excellent heat resistance. Hot aluminum alloy stranded wire.
The tensile strength, conductivity and heat resistance of aluminum alloy strands are improved, ensuring high strength residual rate at high temperatures, reducing resistivity, and enhancing the safety performance and conveying capacity of the line.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloy materials, and in particular to a high-performance heat-resistant aluminum alloy stranded wire and a preparation method thereof. Background Art
[0002] In recent years, the construction of my country's power system has developed rapidly. The transmission environment and working conditions faced by the power transmission area of the power grid are becoming more and more complex. There are more and more large-span conductors across navigable rivers, lakes, straits and high-drop and large-span areas in the mountains. Therefore, higher requirements are put forward for the safety performance and line transmission capacity of large-span conductors. At present, in the construction and transformation of large-span projects, most of them use ordinary steel-core high-strength heat-resistant aluminum alloy stranded wires to replace traditional steel-core high-strength aluminum alloy stranded wires. High-strength heat-resistant aluminum alloy stranded wires effectively increase the transmission capacity of the line, but are limited by the performance of ordinary high-strength heat-resistant aluminum alloys (tensile strength ≥ 225Mpa, resistivity greater than 55% IACS, elongation ≥ 2.0%, continuous heating at 230℃ for 1h or continuous heating at 180℃ for 400h, the strength residual rate of high-strength heat-resistant aluminum alloy stranded wire is greater than 90%), and its strength safety performance needs to be improved, and the resistivity is large, resulting in more line losses. Therefore, it is of great significance to develop a high-performance heat-resistant aluminum alloy stranded wire with high strength, high elongation and high conductivity. Summary of the invention
[0003] In order to solve the above technical problems, the purpose of the present invention is to provide a high-performance heat-resistant aluminum alloy stranded wire and a preparation method thereof, wherein the high-performance heat-resistant aluminum alloy stranded wire has high strength, high elongation, high conductivity and better heat resistance.
[0004] The above object of the present invention is achieved through the following technical solutions:
[0005] A method for preparing a high-performance heat-resistant aluminum alloy stranded wire comprises the following steps:
[0006] S1. The aluminum source is put into a smelting furnace for smelting, and then subjected to boronization treatment to obtain molten aluminum;
[0007] S2. Prepare other raw materials according to the following mass percentages: Fe 0.1-0.2%, Si 0.3-0.6%, Zr 0.1-0.2%, Mg 0.7-0.8%, Er 0.05-0.15%, Ti 0.01-0.02%, Cr+Mn+V 0.0001-0.00055%, B 0.0001-0.0005%, and the rest are Al and other impurity elements, and put the other raw materials into a smelting furnace and smelt them together with the molten aluminum obtained in S1 to obtain alloyed aluminum;
[0008] S3. The alloyed aluminum obtained in S2 is refined to obtain a refined aluminum alloy liquid;
[0009] S4. The refined aluminum alloy liquid obtained in S3 is cast to obtain an aluminum alloy ingot;
[0010] S5. The aluminum alloy ingot obtained in S4 is rolled to obtain an aluminum alloy rod;
[0011] S6. Annealing the aluminum alloy rod obtained in S5 at 200 to 230°C to obtain a high-strength heat-resistant aluminum alloy rod;
[0012] S7. The high-strength heat-resistant aluminum alloy rod obtained in S6 is drawn to obtain a high-strength heat-resistant aluminum alloy wire;
[0013] S8. performing an aging treatment on the high-strength heat-resistant aluminum alloy wire obtained in S7 at 200 to 250° C. to obtain a high-performance heat-resistant aluminum alloy wire;
[0014] S9. The high-performance heat-resistant aluminum alloy wire obtained in S8 is twisted to obtain an initial high-performance heat-resistant aluminum alloy stranded wire;
[0015] S10. The initial high-performance heat-resistant aluminum alloy stranded wire obtained in S9 is annealed at 280-300°C to obtain the high-performance heat-resistant aluminum alloy stranded wire, wherein the high-performance heat-resistant aluminum alloy stranded wire has a tensile strength ≥280MPa, a conductivity ≥57%IACS, an elongation ≥6.0%, and a strength retention rate of ≥97% after continuous heating at 230°C for 1h or continuous heating at 180°C for 400h.
[0016] Furthermore, in S1, the smelting temperature is 720-740°C.
[0017] In a specific implementation, in S1, an aluminum ingot is put into a smelting furnace for smelting, the temperature of the molten aluminum after smelting is 720-740°C, and then a boronization treatment is performed, and 3-4 kg of aluminum-boron alloy is added per ton of molten aluminum.
[0018] Furthermore, in S2, the content of Al is greater than 98%, and other impurity elements are unavoidable impurities.
[0019] In a specific implementation manner, in S2, the molten aluminum in the smelting furnace is put into a holding furnace, and a sample is taken after standing for 30 to 60 minutes. The element content of the sample is quickly analyzed by a spectrometer, and the ingredients are prepared according to the element content results of the sample. After adding other alloys, the molten aluminum is put into the holding furnace again and electromagnetically stirred for 25 to 35 minutes. After standing for 30 to 60 minutes, a sample is taken to obtain Fe0.1-0.2%, Si 0.3-0.6%, Zr 0.1-0.2%, Mg0.7-0.8%, Er 0.05-0.15%, Ti 0.01-0.02%, Cr+Mn+V≤0.00055%, B<0.0005%, and the rest is Al and other impurity elements alloyed aluminum water.
[0020] Among them, Zr, Mg and Si mainly improve the strength of the alloy, but reduce the electrical conductivity of the alloy. Zr can also improve the heat resistance of the alloy; Fe improves the strength of the alloy; Ti and Er will refine the grains, improve thermal stability, and thus improve the heat resistance of the alloy.
[0021] Furthermore, in S3, the refining is performed by nitrogen powder injection refining, and the refining temperature is 700-750°C.
[0022] Furthermore, in S3, the refining time is not less than 30 minutes.
[0023] Furthermore, in S3, after the refining is completed, the mixture is allowed to stand for 30 to 60 minutes, and a sample is taken for spectral analysis. After the composition requirements are met, casting is performed.
[0024] Furthermore, in S4, the casting temperature is 680-720°C, and the casting speed is 6.3-7.5 t / h.
[0025] Furthermore, in S4, cooling water at 25 to 35° C. is used for cooling after casting.
[0026] Furthermore, in S5, the rolling temperature is 500-550°C, and the rolling temperature affects the strength and conductivity of the aluminum alloy rod.
[0027] Furthermore, in S5, an emulsion with a temperature of 50-70°C is used in the rolling, and the temperature of the aluminum alloy rod after rolling is controlled below 100°C.
[0028] Furthermore, in S6, the annealing treatment time is 10 to 15 hours, and the annealing treatment time affects the strength and conductivity of the high-strength heat-resistant aluminum alloy rod.
[0029] Further, in S6, the annealing treatment causes Mg, Si, Zr and Er to precipitate, does not affect the alloy strength, and improves the alloy conductivity. In addition, based on the composition ratio of the present invention and the setting of the above preparation process, the low-temperature annealing treatment at 200-250° C. in S6 can achieve the effect of the high-temperature annealing treatment in the prior art.
[0030] Furthermore, in S7, the drawing speed is 10-16 m / s, and the diameter of the high-strength heat-resistant aluminum alloy wire is 3.00-4.50 mm.
[0031] In a specific implementation, a high-strength heat-resistant aluminum alloy rod is drawn on a non-sliding aluminum alloy wire drawing machine, and a polycrystalline die is used as the wire drawing die.
[0032] Furthermore, in S8, the aging treatment time is 9 to 13 hours, and the aging treatment time affects the strength, conductivity and elongation of the high-performance heat-resistant aluminum alloy wire.
[0033] Furthermore, in S8, the high-strength heat-resistant aluminum alloy wire is subjected to aging treatment, which can improve its electrical conductivity, elongation, heat resistance and other properties. During the aging treatment, dislocations between grains disappear, the single wire strength decreases, but the electrical conductivity increases.
[0034] Furthermore, in S9, a JLK-710 / 12+18+24+30 motor-type frame stranding machine is used to strand the high-performance heat-resistant aluminum alloy conductors. Due to their high strength, residual stress exists during the stranding process. A stress relief device is used to relieve stress on the conductors to ensure that the high-performance heat-resistant aluminum alloy conductors are not loose after stranding.
[0035] During the stranding process, high-performance heat-resistant aluminum alloy conductors pass through multiple guide wheels and rollers, and are twisted and bent many times during the stranding process. The internal structure of the single wire is damaged, which affects the performance of the single wire of the finished conductor, increases the resistivity of the single wire, and reduces the tensile strength, elongation, heat resistance and other properties.
[0036] Furthermore, in S10, the annealing treatment time is 5 to 8 hours.
[0037] Furthermore, in S10, by annealing at high temperature for a short time, the internal structure of the initial high-performance heat-resistant aluminum alloy strand can be improved, making the internal structure uniform and stable, eliminating internal stress, and improving its strength, elongation, heat resistance and conductivity. The present invention also protects the high-performance heat-resistant aluminum alloy strand obtained by the above-mentioned preparation method.
[0038] Beneficial effects of the present invention:
[0039] 1. In the high-performance heat-resistant aluminum alloy stranded wire provided by the present invention, Zr, Mg and Si mainly improve the alloy strength, but reduce the electrical conductivity of the alloy. Zr can also improve the heat resistance of the alloy; Fe improves the alloy strength; Ti and Er refine the grains, improve thermal stability, and thus improve the heat resistance of the alloy.
[0040] 2. In the preparation process provided by the present invention, the high-strength heat-resistant aluminum alloy wire is subjected to aging treatment, which can improve its electrical conductivity, elongation, heat resistance and other properties. During the aging treatment, the dislocation between grains disappears, the single wire strength decreases, but the electrical conductivity increases. Finally, by high-temperature short-time annealing, the internal structure of the initial high-performance heat-resistant aluminum alloy stranded wire can be improved, making its internal structure uniform and stable, eliminating internal stress, and improving its strength, elongation, heat resistance and electrical conductivity. DETAILED DESCRIPTION
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0042] The present invention is further described below in conjunction with specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0043] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0044] The performance of the aluminum alloy stranded wires prepared in the following examples and comparative examples was tested according to GB / T30551-2014.
[0045] Example 1
[0046] A method for preparing a high-performance heat-resistant aluminum alloy stranded wire comprises the following steps:
[0047] S1. Putting aluminum ingots with a grade of Al99.80 into a smelting furnace for smelting, and then performing boronization treatment to obtain smelted aluminum liquid.
[0048] S2. Put the molten aluminum from the smelting furnace into a holding furnace, let it stand for 30 minutes and then take a sample. Use a spectrometer to quickly analyze the element content of the sample, and make the ingredients according to the element content results of the sample. After adding other alloys, put it into the holding furnace again and carry out electromagnetic stirring for 30 minutes. Let it stand for 30 minutes and then take a sample to obtain the alloyed molten aluminum.
[0049] S3. The alloyed aluminum liquid obtained in S2 is refined by nitrogen powder spraying for 40 minutes at a refining temperature of 700°C. After the refining, it is allowed to stand for 30 minutes and samples are taken for spectral analysis to obtain aluminum alloy liquid that meets the composition requirements.
[0050] S4. The aluminum alloy liquid obtained in S3 is continuously cast using a wheel crystallizer, and aluminum-titanium-boron wire is added to the flow trough to refine the grains to obtain an aluminum alloy ingot.
[0051] S5. The aluminum alloy ingot obtained in S4 is sent to the continuous rolling mill through the introduction device, and an aluminum alloy rod with a diameter of 9.5 mm is obtained after rolling. The rod is automatically collected after online cooling.
[0052] S6. The aluminum alloy rod obtained in S5 is annealed at 230°C for 14 hours to allow Mg, Si, Zr and Er elements to be fully precipitated from the matrix, thereby improving the electrical conductivity and obtaining a high-strength heat-resistant aluminum alloy rod.
[0053] S7. The high-strength heat-resistant aluminum alloy rod obtained in S6 was drawn on a non-sliding aluminum alloy wire drawing machine. The wire drawing die used a polycrystalline die. The drawing speed was 15 m / s, and a high-strength heat-resistant aluminum alloy wire with a diameter of 4.21 mm was obtained.
[0054] S8. The high-strength heat-resistant aluminum alloy wire obtained in S7 is subjected to aging treatment at 230°C for 10 hours to obtain a high-performance heat-resistant aluminum alloy wire.
[0055] S9. Use a JLK-710 / 12+18+24+30 motor-type frame stranding machine to strand the high-performance heat-resistant aluminum alloy conductor obtained in S8 to obtain an initial high-performance heat-resistant aluminum alloy stranded wire.
[0056] S10. The initial high-performance heat-resistant aluminum alloy stranded wire obtained in S9 is annealed at 280°C for 5 hours to obtain a high-performance heat-resistant aluminum alloy stranded wire.
[0057] The element contents of the high-performance heat-resistant aluminum alloy stranded wire were measured to be Fe 0.13%, Si 0.42%, Zr 0.16%, Mg 0.77%, Er 0.09%, Ti 0.01%, Cr+Mn+V 0.00043%, B 0.0004%, and the rest were Al and other impurity elements. The tensile strength was 286MPa, the conductivity was 58.4%IACS, the elongation was 6.4%, and the strength retention rate after continuous heating at 230°C for 1h was 98%.
[0058] Example 2
[0059] A method for preparing a high-performance heat-resistant aluminum alloy stranded wire comprises the following steps:
[0060] S1. Putting aluminum ingots with a grade of Al99.80 into a smelting furnace for smelting, and then performing boronization treatment to obtain smelted aluminum liquid.
[0061] S2. Put the molten aluminum from the smelting furnace into a holding furnace, let it stand for 30 minutes and then take a sample. Use a spectrometer to quickly analyze the element content of the sample, and make the ingredients according to the element content results of the sample. After adding other alloys, put it into the holding furnace again and carry out electromagnetic stirring for 30 minutes. Let it stand for 30 minutes and then take a sample to obtain the alloyed molten aluminum.
[0062] S3. The alloyed aluminum liquid obtained in S2 is refined by nitrogen powder spraying for 40 minutes at a refining temperature of 700°C. After the refining, it is allowed to stand for 30 minutes and samples are taken for spectral analysis to obtain aluminum alloy liquid that meets the composition requirements.
[0063] S4. The aluminum alloy liquid obtained in S3 is continuously cast using a wheel crystallizer, and aluminum-titanium-boron wire is added to the flow trough to refine the grains to obtain an aluminum alloy ingot.
[0064] S5. The aluminum alloy ingot obtained in S4 is sent to the continuous rolling mill through the introduction device, and an aluminum alloy rod with a diameter of 9.5 mm is obtained after rolling. The rod is automatically collected after online cooling.
[0065] S6. The aluminum alloy rod obtained in S5 is annealed at 230°C for 13 hours to allow Mg, Si, Zr and Er elements to be fully precipitated from the matrix, thereby improving the electrical conductivity and obtaining a high-strength heat-resistant aluminum alloy rod.
[0066] S7. The high-strength heat-resistant aluminum alloy rod obtained in S6 was drawn on a non-sliding aluminum alloy wire drawing machine. The wire drawing die used a polycrystalline die. The drawing speed was 16 m / s, and a high-strength heat-resistant aluminum alloy wire with a diameter of 3.83 mm was obtained.
[0067] S8. The high-strength heat-resistant aluminum alloy wire obtained in S7 is subjected to aging treatment at 240°C for 11 hours to obtain a high-performance heat-resistant aluminum alloy wire.
[0068] S9. Use a JLK-710 / 12+18+24+30 motor-type frame stranding machine to strand the high-performance heat-resistant aluminum alloy conductor obtained in S8 to obtain an initial high-performance heat-resistant aluminum alloy stranded wire.
[0069] S10. The initial high-performance heat-resistant aluminum alloy stranded wire obtained in S9 is annealed at 285°C for 6 hours to obtain a high-performance heat-resistant aluminum alloy stranded wire.
[0070] The element contents of the high-performance heat-resistant aluminum alloy stranded wire were measured to be Fe 0.15%, Si 0.45%, Zr 0.18%, Mg 0.75%, Er 0.11%, Ti 0.013%, Cr+Mn+V 0.00035%, B 0.0003%, and the rest were Al and other impurity elements. The tensile strength was 290 MPa, the conductivity was 57.1% IACS, the elongation was 6.0%, and the strength retention rate after continuous heating at 230°C for 1 hour was 97%.
[0071] Comparative Example 1
[0072] A method for preparing an aluminum alloy stranded wire comprises the following steps:
[0073] S1. Putting aluminum ingots with a grade of Al99.80 into a smelting furnace for smelting, and then performing boronization treatment to obtain smelted aluminum liquid.
[0074] S2. Put the molten aluminum from the smelting furnace into a holding furnace, let it stand for 30 minutes and then take a sample. Use a spectrometer to quickly analyze the element content of the sample, and make the ingredients according to the element content results of the sample. After adding other alloys, put it into the holding furnace again and carry out electromagnetic stirring for 30 minutes. Let it stand for 30 minutes and then take a sample to obtain the alloyed molten aluminum.
[0075] S3. The alloyed aluminum liquid obtained in S2 is refined by nitrogen powder spraying for 40 minutes at a refining temperature of 700°C. After the refining, it is allowed to stand for 30 minutes and samples are taken for spectral analysis to obtain aluminum alloy liquid that meets the composition requirements.
[0076] S4. The aluminum alloy liquid obtained in S3 is continuously cast using a wheel crystallizer, and aluminum-titanium-boron wire is added to the flow trough to refine the grains to obtain an aluminum alloy ingot.
[0077] S5. The aluminum alloy ingot obtained in S4 is sent to the continuous rolling mill through the introduction device, and an aluminum alloy rod with a diameter of 9.5 mm is obtained after rolling. The rod is automatically collected after online cooling.
[0078] S6. The aluminum alloy rod obtained in S5 was drawn on a non-sliding aluminum alloy wire drawing machine. The wire drawing die used a polycrystalline die. The drawing speed was 15 m / s, and an aluminum alloy wire with a diameter of 4.21 mm was obtained.
[0079] S7. Performing aging treatment on the aluminum alloy wire obtained in S6 at 205° C. for 10 h to obtain a treated aluminum alloy wire.
[0080] S8. Use a JLK-710 / 12+18+24+30 motor-type frame stranding machine to strand the aluminum alloy wire obtained in S7 to obtain an initial aluminum alloy stranded wire.
[0081] S9. The initial aluminum alloy stranded wire obtained in S8 is annealed at 280°C for 5 hours to obtain an aluminum alloy stranded wire.
[0082] The element content of the aluminum alloy stranded wire measured by SPECTRO spectrometer is Fe 0.11%, Si 0.45%, Zr 0.12%, Mg 0.70%, Er 0.06%, Ti 0.014%, Cr+Mn+V 0.00045%, B 0.00047%, the rest are Al and other impurity elements, the tensile strength is 241MPa, the conductivity is 55.8%IACS, the elongation is 3.0%, and the strength retention rate after continuous heating at 230°C for 1h is 92%.
[0083] Comparative Example 2
[0084] A method for preparing an aluminum alloy stranded wire comprises the following steps:
[0085] S1. Putting aluminum ingots with a grade of Al99.80 into a smelting furnace for smelting, and then performing boronization treatment to obtain smelted aluminum liquid.
[0086] S2. Put the molten aluminum from the smelting furnace into a holding furnace, let it stand for 30 minutes and then take a sample. Use a spectrometer to quickly analyze the element content of the sample, and make the ingredients according to the element content results of the sample. After adding other alloys, put it into the holding furnace again and carry out electromagnetic stirring for 30 minutes. Let it stand for 30 minutes and then take a sample to obtain the alloyed aluminum water, in which the Mg and Si components are relatively low.
[0087] S3. The alloyed aluminum liquid obtained in S2 is refined by nitrogen powder spraying for 40 minutes at a refining temperature of 700°C. After the refining, it is allowed to stand for 30 minutes and samples are taken for spectral analysis to obtain aluminum alloy liquid that meets the composition requirements.
[0088] S4. The aluminum alloy liquid obtained in S3 is continuously cast using a wheel crystallizer, and aluminum-titanium-boron wire is added to the flow trough to refine the grains to obtain an aluminum alloy ingot.
[0089] S5. The aluminum alloy ingot obtained in S4 is sent to the continuous rolling mill through the introduction device, and an aluminum alloy rod with a diameter of 9.5 mm is obtained after rolling. The rod is automatically collected after online cooling.
[0090] S6. The aluminum alloy rod obtained in S5 is annealed at 225° C. for 12 h to obtain an annealed aluminum alloy rod.
[0091] S7. The annealed aluminum alloy rod obtained in S6 was drawn on a non-sliding aluminum alloy wire drawing machine. A polycrystalline die was used as the wire drawing die. The drawing speed was 15 m / s to obtain an aluminum alloy wire with a diameter of 4.21 mm.
[0092] S8. Performing aging treatment on the aluminum alloy wire obtained in S6 at 210° C. for 9 hours to obtain a treated aluminum alloy wire.
[0093] S9. Use a JLK-710 / 12+18+24+30 motor-type frame stranding machine to strand the aluminum alloy wire obtained in S7 to obtain an initial aluminum alloy stranded wire.
[0094] S10. The initial aluminum alloy stranded wire obtained in S9 is annealed at 280°C for 5 hours to obtain an aluminum alloy stranded wire.
[0095] The element content of the aluminum alloy stranded wire measured by SPECTRO spectrometer is Fe 0.15%, Si 0.28%, Zr 0.13%, Mg 0.60%, Er 0.10%, Ti 0.016%, Cr+Mn+V 0.00046%, B 0.00035%, the rest are Al and other impurity elements, the tensile strength is 227MPa, the conductivity is 59.2%IACS, the elongation is 4.2%, and the strength retention rate after continuous heating at 230°C for 1h is 94%. The strength is low, but the conductivity is high.
[0096] Comparative Example 3
[0097] A method for preparing an aluminum alloy stranded wire comprises the following steps:
[0098] S1. Putting aluminum ingots with a grade of Al99.80 into a smelting furnace for smelting, and then performing boronization treatment to obtain smelted aluminum liquid.
[0099] S2. Put the molten aluminum from the smelting furnace into a holding furnace, let it stand for 30 minutes and then take a sample. Use a spectrometer to quickly analyze the element content of the sample, and make the ingredients according to the element content results of the sample. After adding other alloys, put it into the holding furnace again and carry out electromagnetic stirring for 30 minutes. Let it stand for 30 minutes and then take a sample to obtain the alloyed molten aluminum.
[0100] S3. The alloyed aluminum liquid obtained in S2 is refined by nitrogen powder spraying for 40 minutes at a refining temperature of 700°C. After the refining, it is allowed to stand for 30 minutes and samples are taken for spectral analysis to obtain aluminum alloy liquid that meets the composition requirements.
[0101] S4. The aluminum alloy liquid obtained in S3 is continuously cast using a wheel crystallizer, and aluminum-titanium-boron wire is added to the flow trough to refine the grains to obtain an aluminum alloy ingot.
[0102] S5. The aluminum alloy ingot obtained in S4 is sent to the continuous rolling mill through the introduction device, and an aluminum alloy rod with a diameter of 9.5 mm is obtained after rolling. The rod is automatically collected after online cooling.
[0103] S6. Annealing the aluminum alloy rod obtained in S5 at 220° C. for 15 h to obtain an annealed aluminum alloy rod.
[0104] S7. The annealed aluminum alloy rod obtained in S6 was drawn on a non-sliding aluminum alloy wire drawing machine. A polycrystalline die was used as the wire drawing die. The drawing speed was 15 m / s to obtain an aluminum alloy wire with a diameter of 4.21 mm.
[0105] S8. Use a JLK-710 / 12+18+24+30 motor-type frame stranding machine to strand the aluminum alloy wire obtained in S7 to obtain an initial aluminum alloy stranded wire.
[0106] S9. The initial aluminum alloy stranded wire obtained in S8 is annealed at 280°C for 5 hours to obtain an aluminum alloy stranded wire.
[0107] The element content of the aluminum alloy stranded wire measured by SPECTRO spectrometer is Fe 0.16%, Si 0.46%, Zr 0.19%, Mg 0.79%, Er 0.10%, Ti 0.018%, Cr+Mn+V 0.00036%, B 0.00043%, the rest are Al and other impurity elements, the tensile strength is 251MPa, the conductivity is 55.2%IACS, the elongation is 2.8%, and the strength retention rate after continuous heating at 230°C for 1h is 90%.
[0108] Comparative Example 4
[0109] A method for preparing an aluminum alloy stranded wire comprises the following steps:
[0110] S1. Putting aluminum ingots with a grade of Al99.80 into a smelting furnace for smelting, and then performing boronization treatment to obtain smelted aluminum liquid.
[0111] S2. Put the molten aluminum from the smelting furnace into a holding furnace, let it stand for 30 minutes and then take a sample. Use a spectrometer to quickly analyze the element content of the sample, and make the ingredients according to the element content results of the sample. After adding other alloys, put it into the holding furnace again and carry out electromagnetic stirring for 30 minutes. Let it stand for 30 minutes and then take a sample to obtain the alloyed molten aluminum.
[0112] S3. The alloyed aluminum liquid obtained in S2 is refined by nitrogen powder spraying for 40 minutes at a refining temperature of 700°C. After the refining, it is allowed to stand for 30 minutes and samples are taken for spectral analysis to obtain aluminum alloy liquid that meets the composition requirements.
[0113] S4. The aluminum alloy liquid obtained in S3 is continuously cast using a wheel crystallizer, and aluminum-titanium-boron wire is added to the flow trough to refine the grains to obtain an aluminum alloy ingot.
[0114] S5. The aluminum alloy ingot obtained in S4 is sent to the continuous rolling mill through the introduction device, and an aluminum alloy rod with a diameter of 9.5 mm is obtained after rolling. The rod is automatically collected after online cooling.
[0115] S6. The aluminum alloy rod obtained in S5 is annealed at 210° C. for 13 h to obtain an annealed aluminum alloy rod.
[0116] S7. The annealed aluminum alloy rod obtained in S6 was drawn on a non-sliding aluminum alloy wire drawing machine. A polycrystalline die was used as the wire drawing die. The drawing speed was 15 m / s to obtain an aluminum alloy wire with a diameter of 4.21 mm.
[0117] S8. The aluminum alloy wire obtained in S7 is subjected to aging treatment at 223° C. for 10.5 h to obtain an aluminum alloy wire.
[0118] S9. Use a JLK-710 / 12+18+24+30 motor-type frame stranding machine to strand the aluminum alloy conductor obtained in S8 to obtain an aluminum alloy stranded wire.
[0119] The element content of the aluminum alloy stranded wire measured by SPECTRO spectrometer is Fe 0.12%, Si 0.51%, Zr 0.17%, Mg 0.74%, Er 0.11%, Ti 0.016%, Cr+Mn+V 0.00033%, B 0.00041%, and the rest are Al and other impurity elements. The tensile strength is 294MPa, the conductivity is 57.1%IACS, the elongation is 4.8%, and the strength retention rate after continuous heating at 230°C for 1h is 94%.
[0120] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a high-performance heat-resistant aluminum alloy stranded wire, characterized in that: The following steps are involved: S1. The aluminum source is put into a smelting furnace for smelting, and then subjected to boronization treatment to obtain molten aluminum; S2. Prepare other raw materials according to the following mass percentages: Fe 0.1-0.2%, Si 0.3-0.6%, Zr 0.1-0.2%, Mg 0.7-0.8%, Er 0.05-0.15%, Ti 0.01-0.02%, Cr+Mn+V 0.0001-0.00055%, B 0.0001-0.0005%, and the rest are Al and other impurity elements, and put the other raw materials into a smelting furnace and smelt them together with the molten aluminum obtained in S1 to obtain alloyed aluminum; S3. The alloyed aluminum obtained in S2 is refined to obtain a refined aluminum alloy liquid; S4. The refined aluminum alloy liquid obtained in S3 is cast, and aluminum-titanium-boron wire is added to obtain an aluminum alloy ingot; S5. The aluminum alloy ingot obtained in S4 is rolled to obtain an aluminum alloy rod; S6. Annealing the aluminum alloy rod obtained in S5 at 200 to 230°C to obtain a high-strength heat-resistant aluminum alloy rod; S7. The high-strength heat-resistant aluminum alloy rod obtained in S6 is drawn to obtain a high-strength heat-resistant aluminum alloy wire; S8. performing an aging treatment on the high-strength heat-resistant aluminum alloy wire obtained in S7 at 200 to 250° C. to obtain a high-performance heat-resistant aluminum alloy wire; S9. The high-performance heat-resistant aluminum alloy wire obtained in S8 is twisted to obtain an initial high-performance heat-resistant aluminum alloy stranded wire; S10. The initial high-performance heat-resistant aluminum alloy stranded wire obtained in S9 is annealed at 280-300°C to obtain the high-performance heat-resistant aluminum alloy stranded wire, wherein the high-performance heat-resistant aluminum alloy stranded wire has a tensile strength ≥280MPa, a conductivity ≥57%IACS, an elongation ≥6.0%, and a strength retention rate of ≥97% after continuous heating at 230°C for 1h or continuous heating at 180°C for 400h.
2. The preparation method according to claim 1, characterized in that: In S1, the smelting temperature is 720-740°C.
3. The preparation method according to claim 1, characterized in that: In S3, the refining is performed by nitrogen powder injection refining at a refining temperature of 700-750°C.
4. The preparation method according to claim 1, characterized in that: In S4, the casting temperature is 680-720°C, and the casting speed is 6.3-7.5 t / h.
5. The preparation method according to claim 1, characterized in that: In S5, the rolling temperature is 500-550°C.
6. The preparation method according to claim 1, characterized in that: In S6, the annealing treatment time is 10 to 15 hours.
7. The preparation method according to claim 1, characterized in that: In S7, the drawing speed is 10-16 m / s, and the diameter of the high-strength heat-resistant aluminum alloy wire is 3.00-4.50 mm.
8. The preparation method according to claim 1, characterized in that: In S8, the aging treatment time is 9 to 13 hours.
9. The preparation method according to claim 1, characterized in that: In S10, the annealing treatment time is 5 to 8 hours.
10. A high performance heat-resistant aluminum alloy stranded wire obtained by the preparation method according to any one of claims 1 to 9.