Electrostatic adsorption mask plate and preparation method thereof

By introducing an electrostatic shielding conductive layer into the electrostatic adsorption mask and grounding, the impact of electrostatic adsorption on gaseous materials and the vulnerability of the mask is solved, which improves the deposition quality and fineness and reduces costs.

CN118932281APending Publication Date: 2024-11-12ANHUI SEMICON INTEGRATED DISPLAY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410903415.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing electrostatic adsorption mask will cause electrostatic adsorption on gaseous molecules, atoms and ions during the vapor deposition process, resulting in problems of blocking holes and uneven deposition, especially on polar molecules and macromolecules, and the mask material is fragile. , it is difficult to meet the needs of high precision and low cost.

Method used

An electrostatic adsorption mask is designed, and an electrostatic shielding conductive layer is used to cover the electrostatic adsorption conductive layer and ground it to shield the electrostatic force lines, preventing it from affecting the movement of gaseous molecules during the vapor deposition process, and ensuring uniform deposition of the material.

Benefits of technology

Effectively shielding the electrostatic force lines, improving the quality and fineness of film deposition, reducing the risk of hole blocking, reducing production costs, and enhancing the mechanical properties of the mask.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932281A_ABST
    Figure CN118932281A_ABST
Patent Text Reader

Abstract

The invention discloses an electrostatic adsorption mask plate and a preparation method thereof. The electrostatic adsorption mask plate comprises a first substrate with a pixel definition layer; the electrostatic adsorption conducting layer is arranged on the first substrate and is used for obtaining electrostatic charges from an external electrostatic generator; the electrostatic shielding conductive layer covers the electrostatic adsorption conductive layer and the surface of the first substrate on the side and is grounded; and the insulating layer is arranged between the electrostatic adsorption conductive layer and the electrostatic shielding conductive layer. When the electrostatic adsorption mask plate provided by the invention is used, the electrostatic shielding conductive layer is grounded, so that a power line can only terminate between the electrostatic shielding conductive layer and the substrate, and the molecular track of a vapor deposition material cannot be influenced, so that the film deposition quality is improved, and the hole blocking risk is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display technology, and in particular to an electrostatic adsorption mask and a preparation method thereof. Background Art

[0002] Vapor deposition technology includes various physical and chemical vapor deposition methods such as thermal evaporation vacuum vapor deposition, magnetron sputtering, molecular beam deposition, chemical vapor deposition and atomic layer deposition. In many fields, including semiconductor and display manufacturing, it is necessary to vapor-deposit a thin film with a specific pattern on a certain substrate. The mask vapor deposition method is to use a film or thin plate with a specific arrangement of holes to block the thin film deposition surface of the substrate during the vapor deposition of the substrate, so that the area blocked by the film or thin plate cannot be deposited with a film, and the film is only deposited in the hole area. This film or thin plate device used to selectively deposit a film on the substrate during the film deposition process is generally called a mask or mask. With the development of high-PPI OLEDOS devices, the development of high-PPI fine masks has become the main research direction of many OLED panels and upstream and downstream manufacturers. In order to improve the accuracy of the pattern, the mask used to make high-precision patterns needs to meet many demanding conditions, mainly including: 1. Very small shadow effect; 2. Appropriate thermal expansion coefficient; 3. Low production, use and cleaning costs.

[0003] Due to the different movement directions of the vapor deposition materials, the edge of the mask away from the substrate will selectively block the vapor phase material, making the thickness of the deposited patterned film uneven, especially the thickness of the edge gradually decreases, resulting in shadows. For fine masks with very small mask patterns, in order to reduce the shadow effect, the thickness of the mask must be very small, which causes the mask to sag significantly under the action of gravity, resulting in a larger gap between the mask and the substrate, which in turn intensifies the shadow effect and reduces the quality of the thin film deposition pattern.

[0004] During the physical and chemical vapor deposition of thin films on a certain substrate, the collision and chemical reaction between the vapor phase material and the substrate surface will cause the substrate and mask to heat up. Some vapor deposition substrates are materials with very low thermal expansion coefficients, such as silicon and glass. The thermal expansion coefficient of silicon is α = 3×10 -6 / K, thermal expansion coefficient of glass α = 7 × 10 -6 / K, at this time, the thermal expansion coefficient is generally 10-20×10 -6 The thermal expansion coefficient of metals between 100 and 200 × 10 -6Materials with too large thermal expansion coefficients, such as polymers with a thermal expansion coefficient between 100 μm and 1 μm, cannot usually be used. This is because for masks that need to produce fine patterns with a size of less than 100 μm or even 1 μm or below, the mismatch in thermal expansion between the mask and the substrate will cause the mask to deform, reduce the quality of the thin film pattern, and cause damage to the mask.

[0005] The materials currently used to make high-precision vapor deposition masks are mainly silicon nitride and Invar alloy, and their thickness is generally only 1-5μm, which makes them very fragile and easily damaged during manufacturing, storage, transportation, use and cleaning, and cannot be used any longer.

[0006] In the prior art, in order to solve the above defects of the traditional fine mask, Liu Chengyuan et al. invented an electrostatic adsorption mask (China Patent Publication No.: CN117385323A). This mask uses a thermal expansion coefficient of 1-3×10 -6 A skeleton made of dielectric materials such as glass or polymer with a low thermal expansion coefficient of 1000 / K is used as a pattern definition layer for vapor deposition. In order to eliminate the droop of the dielectric material, a conductive layer is deposited or pasted on its surface, and an electrostatic generator is used to make the conductive layer statically charged. The pattern definition layer is made to cling to the surface of the substrate through the electrostatic adsorption between the conductive layer and the substrate. Although the problems of low thermal expansion coefficient, low gravity droop and low damage rate of the mask are solved, a bigger problem is introduced at the same time: the electrostatic adsorption has an interaction of attraction or repulsion on all charged substances, including conductors, semiconductors, insulators and plasma in solid, liquid and gaseous states. Therefore, although the electrostatic adsorption mask is clinging to the substrate through the electrostatic adsorption effect, reducing the gravity droop, it will also have an effect on the molecules, atoms, ions and atomic groups deposited in the vapor phase, and even adsorb them in large quantities on the edge surface of the electrostatic adsorption conductive layer, causing blockage and difficulty in depositing on the substrate. This disadvantage is particularly obvious for molecules with large molecular weight and strong induction force and polar molecules. The existing technology cannot solve this problem. Summary of the invention

[0007] In order to solve the problems existing in the prior art, the present invention provides an electrostatic adsorption mask and a preparation method thereof.

[0008] The present invention provides an electrostatic adsorption mask, comprising: a first substrate having a pixel definition layer; an electrostatic adsorption conductive layer, which is arranged on the first substrate and is used to obtain static charge from an external electrostatic generator; an electrostatic shielding conductive layer, which covers the electrostatic adsorption conductive layer and the surface of the first substrate on this side and is grounded; and an insulating layer, which is arranged between the electrostatic adsorption conductive layer and the electrostatic shielding conductive layer.

[0009] Optionally, the electrostatic adsorption mask further includes: an open mask base, and the first substrate is connected to the open mask base.

[0010] Optionally, the first substrate is any one or a combination of glass, silicon nitride, and diamond, and has a thickness ranging from 0.1 to 20 μm.

[0011] Optionally, the electrostatic adsorption conductive layer is made of a conductor or a semiconductor.

[0012] Optionally, the electrostatic shielding conductive layer is made of a conductor or a semiconductor.

[0013] The present invention also provides a method for preparing an electrostatic adsorption mask, comprising: providing a first substrate; forming a patterned electrostatic adsorption conductive layer on a first surface of the first substrate; etching the first substrate using the patterned electrostatic adsorption conductive layer to form a pixel definition layer, wherein the pixel definition layer comprises a plurality of through holes penetrating the first substrate; forming an insulating layer on the surface of the patterned electrostatic adsorption conductive layer; and forming an electrostatic shielding conductive layer on one side of the first surface of the first substrate to cover the surface of the insulating layer and the side walls of the pixel definition layer.

[0014] Optionally, the first substrate is any one or a combination of glass, silicon nitride, and diamond, and has a thickness ranging from 0.1 to 20 μm.

[0015] Optionally, the electrostatic adsorption conductive layer is made of a conductor or a semiconductor.

[0016] Optionally, the electrostatic adsorption shielding layer is made of a conductor or a semiconductor.

[0017] Optionally, the cross-section of the through hole is any one or a combination of a straight through hole, a trapezoidal cross-section through hole, and an inverted trapezoidal cross-section through hole.

[0018] Optionally, the method for preparing the electrostatic adsorption mask also includes: providing a bottom substrate, and before forming an electrostatic adsorption conductive layer on the first surface of the first substrate, connecting the bottom substrate to the second surface of the first substrate through a first bonding layer, the second surface of the first substrate being opposite to the first surface of the first substrate.

[0019] Optionally, forming an insulating layer on the surface of the patterned electrostatic adsorption conductive layer includes: oxidizing the patterned electrostatic adsorption conductive layer with an acidic solution to form an insulating layer on the surface of the patterned electrostatic adsorption conductive layer, corroding the first bonding layer with an acidic solution, and forming pits in the through holes of the pixel definition layer.

[0020] Optionally, the method for preparing the electrostatic adsorption mask further comprises: after forming the electrostatic shielding conductive layer, removing the first bonding layer and the bottom substrate to form the electrostatic adsorption mask.

[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0022] The present invention provides an electrostatic adsorption mask and a preparation method thereof, wherein an electrostatic shielding structure, that is, an electrostatic adsorption conductive layer, is introduced into the electrostatic adsorption mask. By surrounding the electrostatic adsorption conductive layer of the electrostatic adsorption mask with an electrostatic shielding conductive layer and grounding the electrostatic shielding conductive layer, the electric field lines generated during the use of the electrostatic adsorption mask are effectively shielded, so that the electric field lines can only terminate between the electrostatic shielding conductive layer and the substrate without any leakage, and will not affect the deposition of polar gaseous materials on the substrate, thereby increasing the quality of thin film deposition, reducing the risk of hole plugging, and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0024] Figure 1 A schematic diagram of the working principle of an electrostatic adsorption mask without an electrostatic shielding structure in the prior art;

[0025] Figure 2 A schematic diagram of the working principle of an electrostatic adsorption mask according to an embodiment of the present disclosure;

[0026] Figure 3 A schematic diagram of a process for preparing an electrostatic adsorption mask according to an embodiment of the present disclosure;

[0027] Figure 4a-4h A schematic diagram of an intermediate structure of a process for forming an electrostatic adsorption mask according to an embodiment of the present disclosure;

[0028] Figure 5 The cross-sectional structure schematic diagram of the electrostatic adsorption mask of the embodiment of the present disclosure is given as an example;

[0029] Figure 6 The cross-sectional shape schematic diagram of the electrostatic adsorption mask of the embodiment of the present disclosure is given as an example;

[0030] Figure 7 The graph is a comparison of the thickness uniformity of organic material evaporated through an electrostatic adsorption mask without using an electrostatic shielding conductive layer (a) and using an electrostatic shielding conductive layer according to an embodiment of the present disclosure (b). DETAILED DESCRIPTION

[0031] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited to the embodiments set forth herein.

[0032] In the present invention, unless otherwise specified, the directional words used, such as "upper and lower", generally refer to the upper and lower parts of the device in normal use, and "inside and outside" refer to the outline of the device. In addition, the terms "first, second, third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first, second, third" may explicitly or implicitly include one or more of the features. In the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined. In the present invention, it is an electrical device, so connection and interconnection both refer to conductive interconnection. Since the accompanying drawings are descriptions of the same device, the same numbers in the drawings represent the same components.

[0033] As described in the background technology, in the prior art, electrostatic adsorption is used to keep the fine mask close to the substrate during the vapor deposition process, but this will also cause gaseous molecules, atoms or ions to change their trajectories due to the electrostatic effect of the mask. There is a high probability that gaseous molecules will be adsorbed on the sides and surface of the mask, causing problems such as pore blockage and ineffective film coating.

[0034] In the prior art, the process of vapor-depositing organic materials on a silicon-based OLED device by vacuum thermal evaporation under the cover of a mask is taken as an example. Figure 1 As shown, 105 in the figure is the substrate for vapor deposition, that is, the target for the vapor deposition material to be deposited. The anode 106 is generally a transparent indium tin oxide conductive film. 300 represents an organic or inorganic insulating material, which is used to isolate the anode to prevent electrostatic induction between anodes and electrical crosstalk between pixels. 100 represents the skeleton of the electrostatic adsorption mask, which has a series of through holes running through both sides. The vapor deposition material can be deposited on a specific area on the surface of the substrate through these through holes, so that a functional layer with a specific pattern can be deposited on the surface of the substrate. Therefore, this layer of dielectric material is called a pattern definition layer. The electrostatic adsorption conductive layer 101 is connected to an electrostatic generator through an insulated wire, and the surface can carry positive and negative and numerically adjustable electrostatic charges. By adjusting the amount of electrostatic charge, the electrostatic adsorption conductive layer 101 can make the electrostatic adsorption mask plate at 0-75N / cm 2The adjustable force is uniformly adsorbed on the substrate. The dotted line 104 in the figure represents the electric lines of the electrostatic field. For polar molecules 107, the movement in the non-uniform electric field will be affected by the electric field, change the movement trajectory, and even be adsorbed on the surface of the conductive layer, causing uneven coating or even blocking of holes.

[0035] Therefore, the embodiments of the present disclosure provide an electrostatic adsorption mask and a method for preparing the same, so that the electric lines of force can only terminate between the electrostatic shielding layer and the substrate, and will not affect the deposition of polar gaseous materials on the substrate.

[0036] An embodiment of the present disclosure provides an electrostatic adsorption mask, comprising: a first substrate having a pixel definition layer; an electrostatic adsorption conductive layer, disposed on the first substrate, for obtaining static charge from an external electrostatic generator; an electrostatic shielding conductive layer, covering the electrostatic adsorption conductive layer and the surface of the first substrate on this side, and being grounded; and an insulating layer, disposed between the electrostatic adsorption conductive layer and the electrostatic shielding conductive layer.

[0037] The specific examples of the present invention are further described in detail below in conjunction with the accompanying drawings. Among them, the substances not listed in detail in the embodiments can be selected from any substances on the market that can achieve corresponding functions, such as the degumming liquid can be selected from any degumming liquid on the market that can remove the corresponding ultraviolet glue.

[0038] An electrostatic adsorption mask provided by the embodiment of the present disclosure is referred to Figure 2 During the operation of the electrostatic adsorption mask 10, the electrostatic adsorption conductive layer 101 obtains an electrostatic charge with a positive and negative value and a size adjustable in the range of 0.1-300V by connecting to an electrostatic generator. The electrostatic adsorption mask 10 is attached to the substrate 105 through the electrostatic effect, thereby reducing the shadow and other defects during the vapor deposition process; the electrostatic shielding conductive layer 102 is shielded between the electrostatic adsorption conductive layer 101 and the vapor phase material 107, and is grounded through a wire to ensure that the electric line can only terminate between the electrostatic shielding conductive layer 102 and the substrate 105, so that the electric line will not leak, thereby preventing it from affecting the movement trajectory of the gaseous molecules 107 during the vapor deposition process.

[0039] This embodiment also provides a method for preparing an electrostatic adsorption mask, the specific steps are as follows: Figure 3 As shown, Figure 4a-4h The figure shows an intermediate structure diagram of the electrostatic adsorption mask forming process according to an embodiment of the present disclosure. Figure 3 and Figure 4a-4h The preparation method of the electrostatic adsorption mask comprises the following steps:

[0040] S1: providing a first substrate.

[0041] Specifically, a first substrate is provided, which is used as a skeleton of the electrostatic adsorption mask. In some embodiments, the first substrate is any one or a combination of glass, silicon nitride, and diamond. For example, in a specific embodiment, the first substrate can be 1-200 mm in diameter, 0.1-20 μm in thickness, and has a linear expansion coefficient of α=0.1-3×10 -6 Preferably, in the embodiment of the present disclosure, the first substrate has a diameter of 100 mm, a thickness of 10 μm, and a linear expansion coefficient of α=0.1-3×10 -6 / K ultra-thin glass film.

[0042] In some embodiments, the method for preparing the electrostatic adsorption mask further includes: providing a bottom substrate, wherein the bottom substrate is connected to the second surface of the first substrate via a first bonding layer, and the second surface of the first substrate is opposite to the first surface of the first substrate.

[0043] In some embodiments, the bottom substrate is preferably a glass wafer with a diameter of 1-200 mm and a thickness of 0.1-10 mm.

[0044] exist Figure 4a In the embodiment shown, first, the bottom substrate 110 and the first substrate 100 are cleaned with deionized water, acetone and isopropanol for 30 minutes respectively, and then blown dry with ultrapure nitrogen. Afterwards, an aluminum (Al) / lead (Pb) composite film is prepared as the first bonding layer 111 by thermal evaporation on the second surface of the first substrate 100 and the upper surface of the bottom substrate 110, wherein the thickness of the Al material is 50nm and the thickness of the Pb material is 200nm. The lead-plated sides of the two are bonded together by a wafer bonder, the bonding atmosphere is vacuum and formic acid is sprayed to prevent oxidation of the lead surface. After bonding is completed, the two are transferred to a dry engraving machine, and the surface of the first substrate 100 is etched and thinned as a whole. Preferably, the thickness of the first substrate 100 is etched to 5μm or less.

[0045] S3: forming a patterned electrostatic adsorption conductive layer on the first surface of the first substrate.

[0046] like Figure 4b As shown, a magnetron sputtering device is used to form an electrostatically adsorbed conductive layer 101 on the first surface of the first substrate 100. In some embodiments, the material of the electrostatically adsorbed conductive layer 101 can be selected from copper (Cu) / chromium (Cr) / composite film. Preferably, in the embodiment disclosed herein, the Cu film thickness is 20nm and the Cr film thickness is 400nm. Metallic chromium has high hardness and corrosion resistance, and can provide certain support for the glass film as the first substrate 100, increase its toughness and strength, and its linear thermal expansion coefficient is only 5×10 -6 / K, the mask will not fall off during use due to the inconsistency of thermal expansion coefficient with the first substrate 100. Metal copper has low hardness and high ductility, which can increase the adhesion of metal chromium to the first substrate 100 and prevent the chromium layer from peeling off during the production, storage and operation of the mask. The Cu / Cr composite metal film can be connected to an electrostatic generator during the operation of the electrostatic adsorption mask, so that the mask can be tightly adsorbed on a semiconductor or conductor substrate, reducing defects such as shadows during the vapor deposition process.

[0047] In some embodiments, the electrostatically adsorbed conductive layer can have a variety of shapes, structures and numbers of layers. The material of the electrostatically adsorbed conductive layer can be a conductor or semiconductor material with a certain conductivity, and is composed of materials including but not limited to aluminum, copper, titanium, nickel, chromium, tantalum, tungsten, indium tin oxide, zinc oxide, carbon fiber, conductive polymer, heavily doped silicon, semiconductor gallium arsenide, semiconductor perovskite material, organic semiconductor material, etc., or a composite or doped material of one or more of the above.

[0048] Afterwards, if Figure 4c-4d As shown, in this embodiment, a positive photoresist is spin-coated on the surface of the electrostatically adsorbed conductive layer 101, and then exposed and developed to form a patterned first photoresist layer 112; then, the first substrate 100 with a specific pattern of photoresist on the surface is transferred to an ICP etcher together with the bottom substrate 110, and a mixed gas of 30-60sccm Cl2 and 60-90sccm Ar is used to etch the metal material serving as the electrostatically adsorbed conductive layer 101 for 5-10 minutes to form a patterned electrostatically adsorbed conductive layer; then, the patterned first photoresist layer 112 is removed by megasonic cleaning with NMP, deionized water and ethanol and blown dry with nitrogen.

[0049] S5: using the patterned electrostatically adsorbed conductive layer to etch the first substrate to form a pixel definition layer, wherein the pixel definition layer includes a plurality of through holes penetrating the first substrate.

[0050] Reference Figure 4e In a dry etching machine, a mixed gas of 30-60 sccm C4F8 and 60-90 sccm Ar is used to etch the first substrate 100 for 25-30 minutes. The area protected by the patterned electrostatic adsorption conductive layer 101 on the first substrate 100 is not etched, and the through hole 108 is etched in the unprotected area, thereby forming the pixel definition layer of the electrostatic adsorption mask.

[0051] In some embodiments, the cross section of the through hole can be any one or a combination of a straight through hole, a trapezoidal cross section through hole, and an inverted trapezoidal cross section through hole. In the embodiment of the present disclosure, the through hole 108 is an inverted trapezoidal through hole with an inclination angle of 5°. In some other embodiments, the size of the through hole is generally 0.1-20 μm, and the shape of the through hole on the first surface of the first substrate includes but is not limited to various shapes such as circle, quadrilateral, hexagon, octagon and their combinations.

[0052] S7: forming an insulating layer on the surface of the patterned electrostatically adsorbed conductive layer.

[0053] like Figure 4f As shown, in the embodiment of the present disclosure, the first substrate 100 formed with the through hole 108 is transferred together with the bottom substrate 110 into an electrochemical tank, completely immersed in a 2% sulfuric acid aqueous solution, and the Cr of the patterned electrostatically adsorbed conductive layer 101 is anodized using a voltage of 2-10V to generate a 40-60nm dense oxide film on its surface as an insulating layer 103.

[0054] It should be noted that during the anodization process of Cr, the dilute sulfuric acid will homogeneously corrode the first bonding layer 111 of the Al / Pb / Al structure, forming a pit with a substantially circular cross-section in the first bonding layer 111 .

[0055] In the disclosed embodiment, the insulating layer separates the electrostatic adsorption conductive layer from the subsequent electrostatic shielding conductive layer, that is, the insulating layer serves as an isolation structure between the electrostatic adsorption conductive layer and the subsequent electrostatic shielding conductive layer. In some embodiments, the isolation structure is generally required to be an insulating material or semiconductor material with poor conductivity, preferably a composite or doped structure of one or more insulating materials such as silicon oxide, silicon nitride, photoresist, low thermal expansion glass, low thermal expansion polymer, vacuum, etc., but not limited to this. Wherein vacuum means that, in some cases, the gap between the electrostatic adsorption conductive layer and the electrostatic shielding conductive layer is not directly filled with any material, and only the supporting structure of the two in other areas is maintained so as not to attract each other and cause contact.

[0056] In some embodiments, semiconductor materials such as silicon, organic-inorganic hybrid perovskite, and organic semiconductors can also be used as the insulating layer material, but the material or material combination with appropriate resistivity should be selected according to the conductivity of the electrostatic adsorption conductive layer and the electrostatic adsorption voltage to prevent uneven electrostatic adsorption force and thermal deformation of the mask template caused by local overheating caused by leakage current.

[0057] In the disclosed embodiment, the insulating layer is an isolation structure. In some other embodiments, the first substrate used as a skeleton can also be used as an isolation structure, because the thermal expansion coefficient of most conductive materials is difficult to completely match the thermal expansion coefficient of the substrate, especially when single crystal silicon is used as a substrate, due to its very low thermal expansion coefficient, only a very small number of materials such as Invar alloy can meet the demand, and its production, processing and use are also very difficult. In order to increase the selection range of conductive layer materials, materials with a thermal expansion coefficient matching the substrate can be used as a basic skeleton and isolation structure. At this time, the isolation structure with a skeleton function is required to have a thermal expansion coefficient matching the substrate and good mechanical properties. Generally, one or more composite or doped materials such as silicon, silicon oxide, silicon nitride, ordinary glass, low thermal expansion glass, low thermal expansion polyimide, silicon carbide, diamond, aluminum oxide, chromium oxide and other inorganic non-metallic materials, metal oxides, organic materials, etc. are selected.

[0058] S9: forming an electrostatic shielding conductive layer covering the surface of the insulating layer and the sidewalls of the pixel definition layer on one side of the first surface of the first substrate.

[0059] like Figure 4g As shown, in this embodiment, first, the first substrate 100 and the bottom substrate 110 are taken out from the electrochemical tank and washed with deionized water for 10 minutes, dried with nitrogen and placed in a PVD device, and a Cu / Cr composite film is deposited on the first surface of the first substrate 100 by magnetron sputtering as an electrostatic shielding conductive layer 102, wherein the Cu film thickness is preferably 20nm, and the Cr film thickness is preferably 400nm. Since the first bonding layer 111 is etched with pits in step S9, the formed electrostatic shielding conductive layer 102 will not adhere and block the through hole 108.

[0060] In some embodiments, the electrostatic shielding conductive layer can have a variety of shapes, structures and numbers of layers. The material of the electrostatic shielding conductive layer is a conductor or semiconductor material with a certain conductivity, and is composed of materials including but not limited to aluminum, copper, titanium, nickel, chromium, tantalum, tungsten, indium tin oxide, zinc oxide, carbon fiber, conductive polymer, heavily doped silicon, semiconductor gallium arsenide, semiconductor perovskite material, organic semiconductor material, etc., or a composite or doped material of one or more of the above.

[0061] In the embodiment of the present disclosure, after forming the electrostatic shielding conductive layer 102, the first substrate 100 together with the bottom substrate is transferred to 10% hydrochloric acid and soaked for 10 minutes, the first bonding layer between the first substrate 100 and the bottom substrate is removed, the first substrate 100 is taken out, cleaned and dried, and the Figure 4h , a low thermal expansion glass-based electrostatic adsorption mask 10 with an electrostatic shielding structure is formed, wherein the electrostatic shielding structure is the electrostatic shielding conductive layer 102 .

[0062] In the manufacturing process, in order to reduce the shadow effect, the thickness of the fine mask is generally equivalent to the opening size, which reduces the thickness of some fine masks with pixel openings of about 1μm to about 1μm or even sub-micron, making the mask very fragile. In order to enhance the mechanical properties of the fine mask, a substrate of sufficient thickness is generally retained in the non-pixel area of ​​the mask as a reinforcing structure. This structure is generally called reinforcing ribs or reinforcing ribs, generally referred to as ribs. Without these ribs, a mask film with a diameter of several hundred millimeters, a thickness of only a few microns or even less than one micron, and full of holes, will be too fragile to be transferred and used. In addition to retaining a portion of the substrate as a rib, the fine mask generally needs to be pasted on an opening mask made of Invar material welded on a stainless steel frame to further improve the mechanical properties of the fine mask, making it easier to carry, store, use and clean.

[0063] Invar is a nickel-iron alloy that typically contains 36% nickel and 64% iron. It is known for its extremely low coefficient of thermal expansion (CTE), meaning it barely expands or contracts when the temperature changes.

[0064] In some embodiments, the preparation method of the electrostatic adsorption mask template further includes: providing an open mask template with a metal frame, on which a conductive contact is provided; connecting the electrostatic adsorption mask template with the open mask template, wherein one side of the electrostatic shielding conductive layer of the electrostatic adsorption mask template is connected to the open mask template; exposing the welding points of the electrostatic adsorption conductive layer on the electrostatic adsorption mask template through an etching process, and connecting them with the conductive contacts on the metal frame. That is, under the microscope of a manual alignment and pasting device, the electrostatic adsorption mask template is pasted together with an Invar open mask template with a metal frame, and a mask is made by manual equipment and dry etching and other processes are performed to expose the welding points or welding pads of the electrostatic adsorption conductive layer, and then a manual wire bonding machine is used to connect them with the conductive contacts on the metal frame.

[0065] In some embodiments, referring to the structure of a Faraday cage, the electrostatic shielding conductive layer does not have to be a whole and may have certain gaps. Figure 5 Some schematic diagrams of cross-sectional structures of simple electrostatic adsorption masks with electrostatic shielding conductive layers are shown, wherein the electrostatic adsorption conductive layer 101 and the electrostatic shielding conductive layer 102 are both single-layer structures. Figure 6Some schematic examples of the cross-sectional shapes of electrostatic adsorption masks with electrostatic shielding conductive layers are shown. In order to ensure that the mask still has good mechanical properties under the condition of very small shadow effect, it is generally necessary to increase the thickness of its non-functional area as much as possible, and the method includes but is not limited to making through-hole sidewalls with a certain inclination angle, curved sidewalls, or making through-hole sidewalls into stepped structures. In some embodiments, the through-holes formed by etching the first substrate can have various shapes.

[0066] In some embodiments, in order to increase the corrosion resistance and mechanical properties of the electrostatic adsorption mask and reduce the risks of electrostatic breakdown, a passivation layer may be introduced therein. The passivation layer includes but is not limited to an oxide layer formed by in-situ reactions of the electrostatic adsorption conductive layer, the electrostatic shielding conductive layer, the insulating layer and the ribs, and a surface film layer introduced by other means. The in-situ reaction includes but is not limited to in-situ oxidation and fluorination of metals, and the surface film layer introduced by other means includes but is not limited to chemical vapor deposition of silicon nitride, atomic layer deposition of aluminum oxide, chemical electroplating of metals or metal oxides, solution-based surface deposition of polymers, surface sintering of enamel layers, and other surface treatment and protection methods. One or more combinations thereof are not limited in this disclosure.

[0067] In some embodiments, in order to reduce the production cost of the electrostatic adsorption mask or achieve better performance, the production process of the mask includes additive manufacturing and subtractive manufacturing or a hybrid solution thereof. For example, the production process of the pixel definition layer of the electrostatic adsorption mask includes but is not limited to a combination of one or more methods such as chemical reaction in-situ growth, mask vapor deposition, mask solution electroforming deposition, imprinting, model injection molding, printing, mechanical engraving, wet etching, dry etching, laser etching, electron beam etching, ion beam etching, etc., and the present disclosure is not limited thereto.

[0068] The electrostatic adsorption mask containing an electrostatic shielding structure prepared in the embodiment of the present disclosure surrounds the electrostatic adsorption conductive layer and the area outside the vapor deposition substrate through the electrostatic shielding conductive layer. During use, the electrostatic adsorption conductive layer is connected to the electrostatic generator through a wire, and the electrostatic adsorption mask is attached to the substrate through the electrostatic effect, thereby reducing the shadow and other defects during the vapor deposition process. The electrostatic shielding conductive layer is blocked between the electrostatic adsorption conductive layer and the vapor phase material, and is grounded through a wire, so that the electrostatic adsorption conductive layer will not affect the movement of the vapor phase material, which greatly improves the quality of thin film deposition and reduces the plugging speed.

[0069] Using electrostatic adsorption masks without electrostatic shielding structure and with electrostatic shielding structure for C 60 Vacuum thermal evaporation experiment, Figure 7The figure shows the thickness uniformity comparison of the electrostatic adsorption mask without using the electrostatic shielding conductive layer (a) and using the electrostatic shielding conductive layer (b). The thickness of the mask is about 1 μm, the pixel opening width is 2.2 μm, and the C 60 The evaporation thickness is 0.3μm and the electrostatic adsorption voltage is 2V. Figure 7 As shown in the experimental results, the C 60 The pixel shadow width is about 1.2μm, and the thickness uniformity of the organic layer in the pixel area is poor; the C 60 The pixel shadow width is about 0.1 μm, and the thickness uniformity of the organic layer in the pixel area is good.

[0070] Compared with the electrostatic adsorption mask without an electrostatic shielding structure, the electrostatic adsorption mask with an electrostatic shielding structure provided by the present invention surrounds an electrostatic shielding conductive layer outside the electrostatic adsorption conductive layer and grounds the electrostatic shielding conductive layer, so that the electric line can only terminate between the electrostatic shielding layer and the substrate without any leakage, which will not affect the deposition of polar gaseous materials on the substrate, thereby improving the fineness of the mask.

[0071] The above descriptions are merely embodiments of the present application and are not intended to limit the patent scope of the present application. Any equivalent structural or equivalent process transformations made using the contents of the specification and drawings of the present application, such as the mutual combination of technical features between the embodiments, or direct or indirect application in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. An electrostatic adsorption mask, characterized in that: include: a first substrate having a pixel definition layer; An electrostatic adsorption conductive layer, disposed on the first substrate, for obtaining electrostatic charge from an external electrostatic generator; An electrostatic shielding conductive layer covers the electrostatic adsorption conductive layer and the surface of the first substrate on this side and is grounded; The insulating layer is arranged between the electrostatic adsorption conductive layer and the electrostatic shielding conductive layer.

2. The electrostatic adsorption mask according to claim 1, characterized in that: Also includes: An open mask base, wherein the first substrate is connected to the open mask base.

3. The electrostatic adsorption mask according to claim 1, characterized in that: The first substrate is made of any one or a combination of glass, silicon nitride and diamond, and has a thickness ranging from 0.1 to 20 μm.

4. The electrostatic adsorption mask according to claim 1, characterized in that: The material of the electrostatic adsorption conductive layer is a conductor or a semiconductor.

5. The electrostatic adsorption mask according to claim 1, characterized in that: The electrostatic shielding conductive layer is made of a conductor or a semiconductor.

6. A method for preparing an electrostatic adsorption mask, characterized in that: include: providing a first substrate; forming a patterned electrostatically adsorbed conductive layer on the first surface of the first substrate; Etching the first substrate using the patterned electrostatic adsorption conductive layer to form a pixel definition layer, wherein the pixel definition layer includes a plurality of through holes penetrating the first substrate; forming an insulating layer on the surface of the patterned electrostatically adsorbed conductive layer; An electrostatic shielding conductive layer covering the surface of the insulating layer and the side wall of the pixel definition layer is formed on one side of the first surface of the first substrate.

7. The method for preparing an electrostatic adsorption mask according to claim 6, characterized in that: The first substrate is made of any one or a combination of glass, silicon nitride and diamond, and has a thickness ranging from 0.1 to 20 μm.

8. The method for preparing an electrostatic adsorption mask according to claim 6, characterized in that: The material of the electrostatic adsorption conductive layer is a conductor or a semiconductor.

9. The method for preparing an electrostatic adsorption mask according to claim 6, characterized in that: The electrostatic shielding conductive layer is made of a conductor or a semiconductor.

10. The method for preparing an electrostatic adsorption mask according to claim 6, characterized in that: The cross section of the through hole is any one of a straight through hole, a trapezoidal cross section through hole, and an inverted trapezoidal cross section through hole or a combination thereof.

11. The method for preparing an electrostatic adsorption mask according to claim 6, characterized in that: Also includes: A bottom substrate is provided. Before forming an electrostatically adsorbed conductive layer on the first surface of the first substrate, the bottom substrate is connected to the second surface of the first substrate through a first bonding layer. The second surface of the first substrate is opposite to the first surface of the first substrate.

12. The method for preparing an electrostatic adsorption mask according to claim 11, characterized in that: The forming of an insulating layer on the surface of the patterned electrostatic adsorption conductive layer comprises: The patterned electrostatically adsorbed conductive layer is oxidized using an acidic solution to form an insulating layer on the surface of the patterned electrostatically adsorbed conductive layer. The first bonding layer is corroded by using an acidic solution to form a pit in the through hole of the pixel definition layer.