Stainless steel wire for polytetrafluoroethylene hose reinforcement layer and preparation method of stainless steel wire

By optimizing the chemical composition and processing technology of stainless steel wire, including film processing, multi-pass drawing, annealing and pickling, the problem that traditional processes cannot meet the high-strength requirements for aviation are solved, and tensile strength and blowing are prepared. The stainless steel wire with tensile strength of 2200Mpa and above 1300Mpa improves the comprehensive performance of the steel wire.

CN118932326AActive Publication Date: 2024-11-12JIANGYIN FASTEN STAINLESS STEEL PROD CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411187163.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Traditional production processes cannot produce stainless steel wires with tensile strength of not less than 2200Mpa and tensile strength of knotted not less than 1280Mpa, and cannot meet the high strength requirements of aviation hoses.

Method used

Using solid solution pickling HRAP stainless steel strips, the temperature, time and surface reduction ratio of drawing and annealing are controlled through film treatment, multi-pass drawing, annealing, pickling, solid solution treatment, multiple tempering and other process steps, and use Specific lubricating powder and electrolyte ensure high strength of stainless steel wire.

Benefits of technology

The tensile strength of the prepared stainless steel wire is stable at more than 2300Mpa, and the tensile strength of the knot is stable at more than 1300Mpa, which improves the comprehensive performance of the steel wire and reduces the strength loss during braiding or winding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to a stainless steel wire for a polytetrafluoroethylene hose reinforcement layer and a preparation method thereof, and the preparation method comprises the following steps: S1, selecting a stainless steel wire rod subjected to solid solution pickling HRAP, and the chemical composition of the stainless steel wire rod comprises 0.06%-0.08% of C; s2, carrying out membrane treatment; s3, rough extraction; s4, annealing; s5, fine extraction; s6, annealing is conducted; s7, fine drawing; and S8, multiple times of tempering, wherein the stainless steel wire is subjected to reciprocating tempering after fine drawing. According to the preparation method, starting from two aspects of chemical components and a processing technology of stainless steel wire raw materials, it is guaranteed that the tensile strength required by the strength of the stainless steel wire is not smaller than 2300 Mpa, the knotting tensile strength of the steel wire is not smaller than 1300 Mpa, the strength of the packaging steel wire is improved, meanwhile, possible strength loss of a client side in the weaving or winding process is reduced, and the service life of the packaging steel wire is prolonged. The comprehensive performance of the steel wire reinforcement layer is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal wire production and processing, and specifically relates to a stainless steel wire for a polytetrafluoroethylene hose reinforcement layer and a preparation method thereof. Background Art

[0002] Compared with traditional rubber hose assemblies, polytetrafluoroethylene hose assemblies have higher performance requirements, such as light weight, high pressure resistance, aging resistance, corrosion resistance, wide operating temperature range, and long service life. They are widely used in special occasions such as aerospace vehicles, oil drilling, and automobiles. Stainless steel wire is commonly used as the reinforcement layer in polytetrafluoroethylene hose assemblies. The stainless steel wire is arranged on the inner surface of the polytetrafluoroethylene hose in the form of braiding or winding.

[0003] In actual applications, for aviation hoses, since they have to withstand higher temperatures and higher impacts, the tensile strength of the stainless steel wire used in the reinforcement layer of the polytetrafluoroethylene hose is required to be no less than 2200Mpa, and the knotted tensile strength of the steel wire should be no less than 1280Mpa. The performance of stainless steel wire produced by traditional production processes cannot meet the requirements. Summary of the invention

[0004] In view of the above problems, the purpose of the present invention is to provide a method for preparing stainless steel wire for polytetrafluoroethylene hose reinforcement layer, starting from the chemical composition of the stainless steel wire raw materials and the processing technology, to ensure that the strength requirements of the stainless steel wire are not less than 2200Mpa, and the knotted tensile strength of the steel wire should be not less than 1280Mpa.

[0005] The technical solution adopted by the present invention to solve the above problem is: a method for preparing a stainless steel wire for a polytetrafluoroethylene hose reinforcement layer, comprising the following steps: S1: Select the solution pickled HRAP stainless steel wire rod, whose chemical composition is: C: 0.06%~0.08%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.03%, Ni: 8.0%-9.0%, Cr: 18.0%~19.0%, N<0.10%, and the balance is Fe; S2: film treatment, immersing the stainless steel wire rod in step S1 in a film treatment tank containing a film treatment liquid, taking it out and drying it after immersion; S3: Rough drawing, the stainless steel wire rod treated with S2 film is drawn through a straight-through wire drawing machine through a wire pay-off rack for multiple passes to obtain semi-finished stainless steel wire, and then the steel wire is washed with water. Lubricating powder is used in the wire drawing process, and the cooling water temperature of the mold box is 25~35℃; S4: annealing, the semi-finished stainless steel wire obtained in step S3 is first pickled in an electrolytic pickling tank by a passive wire-paying device, then solution treated in a tubular continuous annealing furnace, and finally cooled in a water cooling tank; S5: Fine drawing: the steel wire annealed in step S4 is sequentially drawn through the film tank, oven and straight-in wire drawing machine by the wire pay-off rack for online multi-pass drawing, and then the steel wire is washed with water. Lubricating powder is used in the drawing, and the cooling water temperature of the mold box is 25~35℃; S6: Annealing, the stainless steel wire after fine drawing in S5 is first pickled in an electrolytic acid tank through a passive wire-paying device, then solution treated in a tubular continuous annealing furnace, and finally cooled in a water cooling tank; S7: fine drawing, drawing the stainless steel wire after annealing in step S6 by a water tank wire drawing machine; S8: multiple tempering, the stainless steel wire drawn in step S7 is tempered repeatedly through a tubular furnace.

[0006] Preferably, in step S2, the film treatment liquid is an aqueous solution of a mixture of potassium sulfate and sodium sulfate, the concentration of the film treatment liquid is 15-21wt%, the temperature of the film treatment liquid is 70-90°C, the soaking time is 20-30min; the drying temperature is 180-230°C, and the drying time is 100-150min; Preferably, in step S3, the total surface reduction rate of the stainless steel wire rod drawing is controlled at 70-90%, and except for the last pass using sodium stearate lubricating powder, calcium stearate lubricating powder is used in other passes.

[0007] Preferably, in steps S4 and S6, the stainless steel wire in the electrolytic pickling tank serves as the anode, the lead plate serves as the cathode, and the dilute sulfuric acid solution serves as the electrolyte.

[0008] Preferably, in steps S4 and S6, the solution treatment temperature is 1050-1120°C, and the protective gas is N 2 +H 2 , the heat treatment speed satisfies the wire diameter D×heat treatment speed V=20~25 (mm×m) / min, where the unit of wire diameter is mm and the unit of heat treatment speed is m / min.

[0009] Preferably, in step S5, the total drawing reduction rate is controlled at 70-90%, and the lubricating powder is TF46.

[0010] Preferably, in step S7, the total drawing reduction rate is 91% to 94%, the lubricant is TF486, and the deformation per pass is 13% to 15%.

[0011] Preferably, in step S8, the tempering times are 3 to 5 and the tempering temperature is 180° C. to 220° C.

[0012] A stainless steel wire for a polytetrafluoroethylene hose reinforcement layer is prepared by adopting the preparation method of the stainless steel wire for a polytetrafluoroethylene hose reinforcement layer.

[0013] Compared with the prior art, the advantages of the present invention are: The tensile strength of the stainless steel wire prepared by the preparation method of the present invention is stable at more than 2300Mpa, and the knotting tensile strength is stable at more than 1300Mpa. While the strength of the packaged steel wire is improved, the strength loss that may exist in the weaving or winding of the client is reduced, thereby ensuring the comprehensive performance of the steel wire reinforcement layer. DETAILED DESCRIPTION

[0014] The present invention is further described in detail below with reference to the embodiments. Example 1

[0015] S1: Select φ5.5mm solid solution pickled HRAP stainless steel wire rod, its chemical composition is: C: 0.068%, Si: 0.37%, Mn: 1.23%, P: 0.04%, S: 0.02%, Cr: 18.23%, Ni: 8.06%, N: 0.056%, and the balance is Fe.

[0016] S2: Film treatment. Immerse the φ5.5mm stainless steel wire rod selected in S1 in a film treatment solution at 80℃ for 30 minutes. The film treatment solution is an aqueous solution of potassium sulfate and sodium sulfate with a concentration of 18wt%. After immersion, take it out and place it in a warm air furnace for drying. The drying temperature is 200℃ and the drying time is 120 minutes. Use it after the surface of the steel wire is dry.

[0017] S3: Rough drawing. The φ5.5mm stainless steel wire rod treated with S2 film is drawn through a straight-feed wire drawing machine for 8 passes to obtain semi-finished stainless steel wire. The drawing specifications of each pass are 5.5mm-4.5mm-3.74mm-3.15mm-2.69mm-2.33mm-2.11mm-1.94mm-1.8mm. Except for the last pass, sodium stearate lubricating powder NL305 (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.) is used. Calcium stearate lubricating powder GB205 (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.) is used in other passes. The steel wire is then washed with water to remove the lubricating powder. The cooling water temperature of the mold box is 30℃. The drawing wire specification is φ1.8mm, and the total reduction rate of wire rod drawing is 89.3%.

[0018] S4: Annealing: The semi-finished stainless steel wire is first passed through an electrolytic pickling tank (in which the stainless steel wire is used as anode, the lead plate is used as cathode, and the dilute sulfuric acid solution is used as electrolyte, and the lubricating powder remaining on the surface of the steel wire is removed by electrolytic pickling and water rinsing) through a passive wire-laying device, and then passed through a tubular continuous annealing furnace for solution treatment, and then cooled through a water cooling tank, wherein the solution treatment temperature is 1050°C and the protective gas is N 2 +H 2 , the heat treatment production speed DV is controlled at 20 (mm×m) / min.

[0019] S5: Fine drawing. The steel wire annealed in S4 is drawn online through a wire pay-off rack through a film tank, an oven and a straight-through wire drawing machine in turn for 10 draws. The surface reduction rate of the first drawing is controlled at 25%, and then decreases with each pass. TF46 is used as lubricating powder, and the steel wire is washed with water to remove the lubricating powder. The cooling water temperature of the mold box is 30℃, the steel wire drawing specification is φ0.6mm, and the total surface reduction rate of the steel wire drawing is controlled at 89%.

[0020] S6: Annealing. The stainless steel wire after fine drawing in S5 is first passed through an electrolytic pickling tank (in the electrolytic pickling tank, the stainless steel wire is used as the anode, the lead plate is used as the cathode, and the dilute sulfuric acid solution is used as the electrolyte. The lubricating powder remaining on the surface of the steel wire is removed by electrolytic pickling and water rinsing), and then passed through a tubular continuous annealing furnace for solution treatment, and then cooled through a water cooling tank. The solution treatment temperature is 1050℃ and the protective gas is N 2 +H 2 , the heat treatment production speed DV is controlled at 20 (mm×m) / min.

[0021] S7: Fine drawing: The stainless steel wire annealed in step S6 is drawn by a water tank wire drawing machine. The total drawing reduction rate is 93.75%, the lubricant is TF486, and the deformation per pass is 14%.

[0022] S8: multiple tempering, the stainless steel wire drawn in step S7 is tempered repeatedly through a tubular furnace, the tempering times are 4, and the tempering temperature is 200°C. Example 2

[0023] S1: Select φ5.5mm solid solution pickled HRAP stainless steel wire rod, whose chemical composition is: C: 0.035%, Si: 0.37%, Mn: 1.23%, P: 0.04%, S: 0.02%, Cr: 18.23%, Ni: 8.06%, N: 0.056%, and the balance is Fe.

[0024] S2: Film treatment. Immerse the φ5.5mm stainless steel wire rod selected in S1 in a film treatment solution at 80℃ for 30 minutes. The film treatment solution is an aqueous solution of potassium sulfate and calcium sulfate with a concentration of 18wt%. After immersion, take it out and place it in a warm air furnace for drying. The drying temperature is 200℃ and the drying time is 120 minutes. Use it after the surface of the steel wire is dry.

[0025] S3: Rough drawing. The φ5.5mm stainless steel wire rod treated with S2 film is drawn through a straight-feed wire drawing machine for 6 passes to obtain semi-finished stainless steel wire. The surface reduction rate of the first drawing pass is controlled at 30%, and then decreases according to the passes. Except for the last pass, sodium stearate lubricating powder NL305 (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.) is used. Calcium stearate lubricating powder GB205 (produced by Jiangyin Taifeng Chemical Technology Co., Ltd.) is used in all other passes. The steel wire is then washed with water to remove the lubricating powder. The cooling water temperature of the mold box is 30℃, the specification of the drawn steel wire is 2.55, and the total surface reduction rate of the wire rod drawing is 78.5%.

[0026] S4: Annealing. The semi-finished stainless steel wire is first passed through an electrolytic pickling tank (in which the stainless steel wire is used as anode, the lead plate is used as cathode, and the dilute sulfuric acid solution is used as electrolyte. The lubricating powder remaining on the surface of the steel wire is removed by electrolytic pickling and water rinsing) through a passive wire-laying device, and then passed through a tubular continuous annealing furnace for solution treatment, and then cooled through a water cooling tank. The solution treatment temperature is 1100°C and the protective gas is N 2 +H 2 The heat treatment production speed DV is controlled at 22 (mm×m) / min.

[0027] S5: Fine drawing. The steel wire annealed in S4 is drawn online through a wire pay-off rack through a film tank, an oven and a straight-through wire drawing machine in turn for 9 passes. The surface reduction rate of the first drawing is controlled at 25%, and then decreases with each pass. TF46 is used as lubricating powder, and the steel wire is washed with water to remove the lubricating powder. The cooling water temperature of the mold box is 30℃, the steel wire drawing specification is φ1.0mm, and the total surface reduction rate of the steel wire drawing is controlled at 84.6%.

[0028] S6: Annealing. The stainless steel wire drawn from S5 is first passed through an electrolytic pickling tank (in which the stainless steel wire is used as anode, the lead plate is used as cathode, and the dilute sulfuric acid solution is used as electrolyte. The lubricating powder remaining on the surface of the steel wire is removed by electrolytic pickling and water rinsing) through a passive wire-releasing device, and then passed through a tubular continuous annealing furnace for solution treatment. Finally, it is cooled through a water cooling tank. The solution treatment temperature is 1100°C and the protective gas is N 2 +H 2 The heat treatment production speed DV is controlled at 22 (mm×m) / min.

[0029] S7: Fine drawing: The stainless steel wire annealed in step S6 is drawn by a water tank wire drawing machine. The total reduction rate of drawing is 91.59%, the lubricant is TF486, and the deformation per pass is 15%.

[0030] S8: multiple tempering, the stainless steel wire drawn in step S7 is tempered repeatedly through a tubular furnace, the tempering times are 3 times, and the tempering temperature is 220°C.

[0031] Comparative Example 1 Compared with Example 1, the only difference is that in step S1, φ5.5 mm solid solution pickled HRAP stainless steel wire rod is selected, and its chemical composition is: C: 0.035%, Si: 0.37%, Mn: 1.23%, P: 0.04%, S: 0.02%, Cr: 18.23%, Ni: 8.06%, N: 0.056%, and the remainder is Fe.

[0032] Comparative Example 2 Compared with Example 1, the only difference is that in step S1, φ5.5 mm hot-rolled pickled HRP stainless steel wire rod is selected, and its chemical composition is: C: 0.068%, Si: 0.37%, Mn: 1.23%, P: 0.04%, S: 0.02%, Cr: 18.23%, Ni: 8.06%, N: 0.056%, and the remainder is Fe.

[0033] Comparative Example 3 Compared with Example 1, the only difference is that the S8 multiple tempering step is not performed.

[0034] Comparative Example 4 Compared with Example 1, the only difference is that in the S5 fine drawing step, the steel wire drawing specification is φ0.45 mm, and the total wire drawing reduction rate is controlled at 93.75%; and in the S7 fine drawing step, the total drawing reduction rate is 89%.

[0035] The same test method was used to test the tensile strength and knotting tensile strength of Examples 1-2 and Comparative Examples 1-4. The results are shown in the following table:

[0036] In addition to the above embodiments, the present invention also includes other implementation modes. Any technical solutions formed by equivalent transformation or equivalent replacement should fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing a stainless steel wire for a polytetrafluoroethylene hose reinforcement layer, characterized in that: The following steps are involved: S1: Select the solution pickled HRAP stainless steel wire rod, whose chemical composition is: C: 0.06%~0.08%, Si≤1.00%, Mn≤2.00%, P≤0.045%, S≤0.03%, Ni: 8.0%-9.0%, Cr: 18.0%~19.0%, N<0.10%, and the balance is Fe; S2: film treatment, immersing the stainless steel wire rod in step S1 in a film treatment tank containing a film treatment liquid, taking it out and drying it after immersion; S3: Rough drawing, the stainless steel wire rod treated with S2 film is drawn through a straight-through wire drawing machine through a wire pay-off rack for multiple passes to obtain semi-finished stainless steel wire, and then the steel wire is washed with water. Lubricating powder is used in the wire drawing process, and the cooling water temperature of the mold box is 25~35℃; S4: annealing, the semi-finished stainless steel wire obtained in step S3 is first pickled in an electrolytic pickling tank by a passive wire-paying device, then solution treated in a tubular continuous annealing furnace, and finally cooled in a water cooling tank; S5: Fine drawing: the steel wire annealed in step S4 is sequentially drawn through the film tank, oven and straight-in wire drawing machine by the wire pay-off rack for online multi-pass drawing, and then the steel wire is washed with water. Lubricating powder is used in the drawing, and the cooling water temperature of the mold box is 25~35℃; S6: Annealing, the stainless steel wire after fine drawing in S5 is first pickled in an electrolytic acid tank through a passive wire-paying device, then solution treated in a tubular continuous annealing furnace, and finally cooled in a water cooling tank; S7: fine drawing, drawing the stainless steel wire after annealing in step S6 by a water tank wire drawing machine; S8: multiple tempering, the stainless steel wire drawn in step S7 is tempered repeatedly through a tubular furnace.

2. The method for preparing the stainless steel wire for the reinforcing layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In step S2, the film treatment liquid is an aqueous solution of a mixture of potassium sulfate and sodium sulfate, the concentration of the film treatment liquid is 15~21wt%, the temperature of the film treatment liquid is 70~90℃, the immersion time is 20~30min; the drying temperature is 180~230℃, and the drying time is 100~150min.

3. The method for preparing the stainless steel wire for the reinforcement layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In step S3, the total surface reduction rate of stainless steel wire rod drawing is controlled at 70-90%. Except for the last pass using sodium stearate lubricating powder, calcium stearate lubricating powder is used in other passes.

4. The method for preparing the stainless steel wire for the reinforcement layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In steps S4 and S6, the stainless steel wire in the electrolytic pickling tank is used as the anode, the lead plate is used as the cathode, and the dilute sulfuric acid solution is used as the electrolyte.

5. The method for preparing the stainless steel wire for the reinforcement layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In steps S4 and S6, the solution treatment temperature is 1050~1120°C, the protective gas is N2+H2, and the heat treatment speed satisfies the wire diameter D×heat treatment speed V=20~25 (mm×m) / min, where the unit of the wire diameter is mm and the unit of the heat treatment speed is m / min.

6. The method for preparing the stainless steel wire for the reinforcement layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In step S5, the total drawing reduction rate is controlled at 70-90%, and TF46 is used as lubricating powder.

7. The method for preparing the stainless steel wire for the reinforcement layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In step S7, the total drawing reduction rate is 91% to 94%, the lubricant is TF486, and the deformation per pass is 13% to 15%.

8. The method for preparing the stainless steel wire for the reinforcement layer of the polytetrafluoroethylene hose according to claim 1, characterized in that: In step S8, the tempering times are 3 to 5 and the tempering temperature is 180°C to 220°C.

9. A stainless steel wire for a polytetrafluoroethylene hose reinforcement layer, characterized in that: The polytetrafluoroethylene hose reinforcement layer is prepared by the method for preparing stainless steel wire for the polytetrafluoroethylene hose reinforcement layer according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Wiredrawing process of stainless steel wire for glasses frame

    CN113198860A

  • Preparation method of 1Cr18Ni9Ti high-strength high-plasticity cold heading wire and steel wire

    CN115747615A

  • Destressing heat treatment method for 304H austenitic stainless steel wire

    CN117604235A

  • Preparation method for stainless steel wire for netting

    WO2023035443A1

  • Stainless steel wire and preparation method therefor, and stainless steel spring

    WO2023035444A1