Oxygen evolution catalyst for AEM water electrolysis hydrogen production and preparation method of oxygen evolution electrode
Through hydrothermal method and LDH sheet control agent, combined with binder and rolling technology, the problem of insufficient electrode firmness and loading in the preparation of iron-cobalt nickel-LDH catalyst is solved, and high-performance FeCoNi suitable for industrial production is achieved. -LDH electrode.
Patent Information
- Application Number
- CN202410898075.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing iron-cobalt nickel-LDH catalyst preparation methods, self-supported in-situ growth method and electrodeposition method lead to poor electrode firmness, low loading of active substances, poor repeatability, and high cost of precious metal catalysts, which limits the large-scale application of hydrogen energy. .
The FeCoNi-LDH catalyst was prepared by hydrothermal method, and a single-layer structure was prepared by medium and low temperature liquid phase control and LDH sheet control agent, combining binder and rolling technology to improve the firmness and loading of the electrode.
A FeCoNi-LDH catalyst with high purity, uniform particle size and good dispersion was obtained, and the electrode coating has improved firmness and extended life. It is suitable for large-scale industrial production, and the electrochemical performance and durability are improved.
Smart Images

Figure CN118932380A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, and in particular to a method for preparing an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis hydrogen production. Background Art
[0002] As an ideal clean energy, hydrogen is considered to be one of the energy sources with broad development prospects in the future. Among hydrogen production technologies, anion exchange membrane (AEM) hydrogen production technology can combine the advantages of high current density of solid electrolyte (PEM) hydrogen production and low cost of alkaline water electrolysis (ALK) technology, and is considered to be the most promising technology for large-scale hydrogen production in the future.
[0003] The core reaction of hydrogen production by water electrolysis is two spatially independent half-reactions, including the oxygen evolution reaction (OER) with four electron transfer at the anode and the hydrogen evolution reaction (HER) with two electron transfer at the cathode. Among them, the reaction energy barrier and slow electron transfer rate in the four-electron OER process make it the main problem for the widespread application of water splitting. The use of catalysts can effectively alleviate these problems. Today, iridium (Ir), ruthenium (Ru) and their oxides are considered to be the most effective catalysts for catalyzing OER. However, the natural reserves of precious metals are low and the cost of use is high. Large-scale application will greatly increase the production cost of hydrogen energy, which is not conducive to the development of hydrogen energy. Therefore, the development of environmentally friendly, naturally abundant, low-cost and high-performance electrocatalysts to replace precious metal catalysts is of great significance for the large-scale application of electrochemical water splitting.
[0004] Iron-cobalt-nickel transition metal layered double hydroxide (FeCoNi-LDH) has shown potential industrial value in AEM catalysts due to its excellent intrinsic catalytic activity, special structure and high catalytic activity in alkaline environment.
[0005] At present, the methods for preparing FeCoNi-LDH catalysts are mainly immersion in-situ growth method, hydrothermal in-situ growth method and electrodeposition method, such as patent number CN115386908A: a FeCoNi double hydroxide nanocage electrocatalytic oxygen evolution material and its preparation method, the preparation method is immersion in-situ growth method, that is, the foamed nickel is immersed in a cobalt salt aqueous solution, and then a 2-methylimidazole aqueous solution is added, and the soaking is continued, and finally the MOF precursor is immersed in a mixed aqueous solution containing Fe salt, Ni salt and urea. For example, patent CN114892207A: a NiFeCo-LDH / NF electrocatalyst and its preparation method, the preparation method is electrodeposition method, first pre-treating the foamed nickel, and then preparing the FeCoNi precursor electroplating solution, immersing the foamed nickel as a cathode in the electroplating solution, applying a certain voltage for electroplating, after the electroplating is completed, the foamed nickel is taken out, rinsed with deionized water, and dried at 60°C to obtain the NiFeCo-LDH / NF electrocatalyst. For example, patent invention CN111495417B: A nickel foam loaded with iron, cobalt and nickel metal nanocatalyst and its preparation method and application. The preparation method is a hydrothermal in-situ growth method, in which the nickel foam is cut and pretreated for use; three metal salts of cobalt nitrate, ferrous nitrate and nickel nitrate, ammonium fluoride and urea are dissolved in deionized water, stirred to obtain a hydrothermal solution, and then the pretreated nickel foam and the prepared hydrothermal solution are added to a high-pressure reactor, and the high-pressure reactor is placed in a forced air drying oven for hydrothermal reaction.
[0006] At present, the preparation of iron-cobalt-nickel-LDH catalyst by the methods of impregnation in-situ growth, hydrothermal in-situ growth and electrodeposition is simple in preparation process, and the OER electrode can be prepared in one step. The prepared electrode does not need to add other additives such as binders to avoid affecting the OER performance of the electrode. However, there are still the following disadvantages: in actual use, the electrodes prepared by the self-supporting in-situ growth method and the electrodeposition method have poor firmness, and the surface catalyst will leach out and fall off, especially under the condition of being squeezed during stacking, which will affect the life and performance. In addition, the electrode active material loading of the self-supporting in-situ growth method and the electrodeposition method is low, and the loading is difficult to control, which will affect the long-term durability of the electrode. The prepared electrode has poor reproducibility and is not suitable for large-scale industrial production. In addition, the prepared iron-cobalt-nickel-LDH is a multilayer structure with fewer active sites and poor performance. Summary of the invention
[0007] Based on the technical problems existing in the background technology, the present invention proposes a preparation method of an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis to produce hydrogen.
[0008] The present invention provides a method for preparing an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis hydrogen production, comprising:
[0009] S1, dissolving a mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating the mixture to obtain an iron-cobalt-nickel precursor;
[0010] S2, adding a precipitant to the iron-cobalt-nickel precursor, performing secondary stirring and secondary ultrasonic treatment, wherein the precipitant includes one or more of KOH, NaOH, Na2CO3, NaHCO3, sodium citrate, organic amines, ammonia water or urea;
[0011] S3, adding an LDH layer control agent to obtain a mixed solution; wherein the layer control agent is one or more of formamide, dimethylformamide, and dimethylacetamide;
[0012] S4, adding the mixed solution into a hydrothermal reaction kettle;
[0013] S5, tightening the hydrothermal reactor and setting the hydrothermal reaction temperature and reaction time;
[0014] S6, cooling to room temperature, and filtering the liquid after the reaction to obtain a precipitate;
[0015] S7, washing and drying the precipitate to obtain FeCoNi-LDH catalyst powder;
[0016] S8, mixing the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them to a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry;
[0017] S9, evenly coating the slurry on a preset nickel foam surface, and placing it in a drying oven for drying to obtain a FeCoNi-LDH / NF sample;
[0018] S10, rolling the FeCoNi-LDH / NF sample by a preset rolling press to obtain a FeCoNi-LDH / NF electrode.
[0019] Furthermore, the step of dissolving the mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating to obtain an iron-cobalt-nickel precursor further includes:
[0020] The mass molar ratio of the iron salt, the cobalt salt and the nickel salt is 1-5:1:1-5.
[0021] Furthermore, the step of adding the mixed solution into the hydrothermal reaction kettle further comprises:
[0022] The mass molar ratio of metal ions to precipitants in the mixed solution is 1:0.2-5.
[0023] Furthermore, the steps of fastening the hydrothermal reactor and setting the hydrothermal reaction temperature and reaction time also include:
[0024] The hydrothermal reaction temperature is 80°C-160°C, and the reaction time is 4h-8h.
[0025] Furthermore, the step of washing and drying the precipitate to obtain FeCoNi-LDH catalyst powder further includes:
[0026] The precipitate was washed several times with deionized water and ethanol.
[0027] Furthermore, before the step of mixing the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry, the step further comprises:
[0028] The preset nickel foam was immersed in HCl, anhydrous ethanol and deionized water respectively, ultrasonically cleaned for multiple times, and dried.
[0029] Furthermore, the step of immersing the preset nickel foam in HCl, anhydrous ethanol and deionized water respectively, performing ultrasonic cleaning multiple times, and drying also includes:
[0030] Each cleaning time is 10 minutes.
[0031] Furthermore, the step of mixing the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry further includes:
[0032] The mass molar ratio of the FeCoNi-LDH catalyst powder, the binder, the dispersant, the organic solvent and the deionized water is 10-40:1-10:1-5:45-88, wherein the binder is one or more of AEM membrane solution, PTFE emulsion, PVDF, acrylic resin, and carboxymethyl cellulose; and the dispersant is one or more of metal phosphate, sodium dodecyl sulfate, polyethylene glycol, and polyacrylamide.
[0033] Furthermore, the step of uniformly coating the slurry on a preset nickel foam surface and placing it in a drying box for drying further includes:
[0034] The coating method is one or more of spray coating, brush coating, comma blade coating, wire rod coating, and slit extrusion coating;
[0035] The drying time of the drying box is 0.5h-2h.
[0036] Furthermore, the step of rolling the FeCoNi-LDH / NF sample by a roller press to obtain a FeCoNi-LDH / NF electrode comprises:
[0037] The roller press pressure is 2t-20t, and the roller pressing thickness is 0.1mm-0.5mm.
[0038] The present invention has the following beneficial effects:
[0039] The FeCoNi-LDH catalyst is prepared by a hydrothermal method, which uses medium and low temperature liquid phase control. The process is relatively simple and does not require high temperature treatment to obtain a product with complete crystal form, uniform particle size distribution and good dispersibility. The obtained product has uniform phase, high purity, good crystallization, high yield, and controllable morphology and size. The obtained FeCoNi-LDH catalyst has high repeatability and good electrochemical performance and can be suitable for large-scale industrial production. By changing the reaction temperature, pressure and reaction time, the reaction and crystal growth can be effectively controlled during the hydrothermal process.
[0040] The present invention adds an LDH layer control agent to prepare a single-layer FeCoNi-LDH, which contains more oxygen evolution active sites, has a larger specific surface area and higher electrocatalytic performance.
[0041] The prepared FeCoNi-LDH / NF electrode uses a binder to fix the catalyst on the surface of the nickel foam, and the catalyst, binder and nickel foam are squeezed more tightly and firmly by rolling, which can prevent the coating from falling off, making the electrode coating more firm and longer in service life. Compared with the self-supporting in-situ growth method and the electrodeposition method, the invention can regulate the loading amount of the FeCoNi-LDH / NF electrode and can have a higher loading amount. The higher loading amount can not only improve the electrochemical performance, but also improve the durability of the electrode for long-term use. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 The present invention provides a process flow chart of a method for preparing an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis hydrogen production;
[0043] Figure 2 This is a scanning electron microscope image of the FeCoNi-LDH catalyst prepared in Example 1 of the present invention;
[0044] Figure 3 The linear sweep voltammograms of Example 1, Example 2, Example 3 and Comparative Example 1 of the present invention are shown;
[0045] Figure 4For Example 1 and Comparative Example 1, the constant current was 800 mA / cm 2 The potential-time curve at . DETAILED DESCRIPTION
[0046] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0048] Refer to the attached Figure 1 , a method for preparing an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis hydrogen production, comprising:
[0049] S1, dissolving a mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating the mixture to obtain an iron-cobalt-nickel precursor;
[0050] S2, adding a precipitant to the iron-cobalt-nickel precursor, performing secondary stirring and secondary ultrasonic treatment, wherein the precipitant includes one or more of KOH, NaOH, Na2CO3, NaHCO3, sodium citrate, organic amines, ammonia water or urea;
[0051] S3, adding an LDH layer control agent to obtain a mixed solution; wherein the layer control agent is one or more of formamide, dimethylformamide, and dimethylacetamide;
[0052] S4, adding the mixed solution into a hydrothermal reactor;
[0053] S5, tighten the hydrothermal reactor and set the hydrothermal reaction temperature and reaction time;
[0054] S6, cooling to room temperature, and filtering the liquid after the reaction to obtain a precipitate;
[0055] S7, washing and drying the precipitate to obtain FeCoNi-LDH catalyst powder;
[0056] S8, mixing FeCoNi-LDH catalyst powder, a binder, a dispersant, an organic solvent and deionized water, adding the mixture to a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry;
[0057] S9, evenly coating the slurry on a preset nickel foam surface, and placing it in a drying oven for drying to obtain a FeCoNi-LDH / NF sample;
[0058] S10, rolling the FeCoNi-LDH / NF sample by a preset rolling press to obtain a FeCoNi-LDH / NF electrode.
[0059] In the above steps, a FeCoNi-LDH catalyst powder is first prepared by a hydrothermal method, wherein FeCoNi-LDH is an iron-cobalt-nickel layered double hydroxide, and LDH is layered double hydroxides, which is a material with a layered structure and is formed by combining two or more metal hydroxides; then the FeCoNi-LDH catalyst powder is prepared into a slurry and coated on the surface of nickel foam, and then the FeCoNi-LDH / NF electrode is prepared by hot pressing, wherein the FeCoNi-LDH / NF electrode is an oxygen evolution electrode of an iron-cobalt-nickel transition metal layered double hydroxide based on nickel foam. Specifically, the preparation process of the FeCoNi-LDH catalyst is as follows: dissolving a mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating the mixture so that the mixture is evenly mixed with the deionized water, and obtaining an iron-cobalt-nickel precursor, wherein the ultrasonic treatment is to treat an object using ultrasonic waves, and the precursor is a form that exists before obtaining the target product, usually in the form of an organic and inorganic complex or a mixture solid, and sometimes in the form of a sol; then adding a precipitant to the iron-cobalt-nickel precursor, performing secondary stirring and secondary ultrasonic treatment, wherein the precipitant includes one or more of KOH, NaOH, Na2CO3, NaHCO3, sodium citrate, organic amines, ammonia water or urea; then adding a certain amount of LDH flake controller to obtain a mixed solution; wherein the flake controller is one or more of formamide, dimethylformamide and dimethylacetamide; adding the LDH flake controller can prepare a single-layer FeCoNi-LDH with a higher specific surface area and higher electrocatalytic performance. Then, the mixed solution is added into the hydrothermal reactor, and then the hydrothermal reactor is tightened, and the hydrothermal reaction temperature and reaction time are set; after the reaction is completed, it is cooled to room temperature, and then the liquid after the reaction is poured out, and then filtered to obtain a precipitate; then the filtered precipitate is washed and dried to obtain FeCoNi-LDH catalyst powder; the FeCoNi-LDH catalyst is prepared by a hydrothermal method, and medium and low temperature liquid phase control is adopted, the process is relatively simple, and a product with complete crystal form, uniform particle size distribution and good dispersibility can be obtained without high temperature treatment, and the obtained product has uniform phase, high purity, good crystallization, high yield, and controllable morphology and size; the obtained FeCoNi-LDH catalyst has high repeatability and good electrochemical performance, and can be suitable for large-scale industrial production; by changing the reaction temperature, pressure and reaction time, the reaction and crystal growth can be effectively controlled in the hydrothermal process.Then, FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water are mixed and added to a planetary mixer, a ball mill, a degassing machine or a high-speed disperser for long-term stirring to obtain a uniform slurry; the prepared slurry is evenly coated on the pretreated nickel foam surface, and placed in a drying oven for drying to obtain a FeCoNi-LDH / NF semi-finished product, and then the dried FeCoNi-LDH / NF semi-finished product is rolled by a roller press to obtain a FeCoNi-LDH / NF electrode. The prepared FeCoNi-LDH / NF electrode uses a binder to fix the catalyst on the nickel foam surface, and the catalyst, binder and nickel foam are squeezed more tightly and firmly by rolling, which can prevent the coating from falling off, making the electrode coating more firm and longer in life; compared with the self-supporting in-situ growth method and the electrodeposition method, the invention can regulate the loading amount of the FeCoNi-LDH / NF electrode, and can have a higher loading amount, which can not only improve the electrochemical performance, but also improve the durability of the electrode for long-term use.
[0060] In this embodiment, the step of dissolving a mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating the mixture to obtain an iron-cobalt-nickel precursor further includes:
[0061] The mass molar ratio of the iron salt, the cobalt salt and the nickel salt is 1-5:1:1-5.
[0062] The step of adding the mixed solution into the hydrothermal reaction kettle also includes:
[0063] The mass molar ratio of metal ions to precipitants in the mixed solution is 1:0.2-5.
[0064] The steps of fastening the hydrothermal reactor and setting the hydrothermal reaction temperature and reaction time also include:
[0065] The hydrothermal reaction temperature is 80°C-160°C, and the reaction time is 4h-8h.
[0066] The step of washing and drying the precipitate to obtain FeCoNi-LDH catalyst powder also includes:
[0067] The precipitate was washed several times with deionized water and ethanol.
[0068] In the specific implementation, a mixture of iron salt, cobalt salt and nickel salt is dissolved in deionized water, and stirred and ultrasonically treated to obtain an iron-cobalt-nickel precursor, wherein the mass molar ratio of the iron salt, the cobalt salt and the nickel salt is 1-5:1:1-5; a precipitant is added to the iron-cobalt-nickel precursor, and secondary stirring and secondary ultrasonic treatment are performed, and then an LDH layer control agent is added to obtain a mixed solution, and then the mixed solution is added to a hydrothermal reactor, wherein the mass molar ratio of metal ions to the precipitant in the mixed solution is 1:0.2-5; then the hydrothermal reactor is tightened, and the hydrothermal reaction temperature and reaction time are set, wherein the hydrothermal reaction temperature is 80°C-160°C, and the reaction time is 4h-8h; it is cooled to room temperature, and the reacted liquid is filtered to obtain a precipitate, and then the precipitate is washed and dried with deionized water and ethanol to obtain a FeCoNi-LDH catalyst powder.
[0069] In this embodiment, before the step of mixing FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry, the step further includes:
[0070] The preset nickel foam was immersed in HCl, anhydrous ethanol and deionized water respectively, ultrasonically cleaned for multiple times, and dried.
[0071] The steps of immersing the preset nickel foam in HCl, anhydrous ethanol and deionized water respectively, performing ultrasonic cleaning for multiple times, and drying also include:
[0072] Each cleaning time is 10 minutes.
[0073] The step of mixing FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry also includes:
[0074] The mass molar ratio of FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water is 10-40:1-10:1-5:45-88, wherein the binder is one or more of AEM membrane solution, PTFE emulsion, PVDF, acrylic resin and carboxymethyl cellulose; the dispersant is one or more of metal phosphate, sodium dodecyl sulfate, polyethylene glycol and polyacrylamide.
[0075] The step of uniformly coating the slurry on a preset nickel foam surface and placing the slurry in a drying oven for drying also includes:
[0076] The coating method is one or more of spray coating, brush coating, comma blade coating, wire rod coating, and slot extrusion coating;
[0077] The drying time of the drying oven is 0.5h-2h.
[0078] The step of rolling the FeCoNi-LDH / NF sample by a roller press to obtain a FeCoNi-LDH / NF electrode comprises:
[0079] The roller press pressure is 2t-20t, and the roller pressing thickness is 0.1mm-0.5mm.
[0080] In the specific implementation, the AEM membrane solution is an anion exchange membrane solution, wherein AEM is Anion Exchange Membrane; the PTFE emulsion is a polytetrafluoroethylene emulsion, wherein PTFE is Polytetrafluoroethylene; and PVDF is polyvinylidene difluoride. First, the preset nickel foam is immersed in HCl, anhydrous ethanol and deionized water respectively, and ultrasonic cleaning is performed for multiple times, each cleaning for 10 minutes, and then it is dried for use; then the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water are mixed and added to a planetary mixer, a ball mill, a degassing machine or a high-speed disperser for stirring, and a slurry is obtained after uniform stirring, wherein the mass molar ratio of the FeCoNi-LDH catalyst powder, the binder, the dispersant, the organic solvent and the deionized water is 10-40: 1-10: 1-5: 45-88, wherein the binder is AEM membrane solution, PTFE emulsion, PVDF, acrylic One or more of acrylic resin and carboxymethyl cellulose; the dispersant is one or more of metal phosphate, sodium dodecyl sulfate, polyethylene glycol and polyacrylamide; then the prepared slurry is evenly coated on the pretreated nickel foam surface by spraying, brushing, comma blade coating, wire rod coating and slit extrusion coating; and the slurry is placed in a drying oven for drying for 0.5h-2h to obtain a FeCoNi-LDH / NF sample, and then the dried FeCoNi-LDH / NF sample is placed in a roller press for roller pressing to obtain a FeCoNi-LDH / NF electrode, wherein the roller press pressure is 2t-20t and the roller pressing thickness is 0.1mm-0.5mm. The prepared FeCoNi-LDH / NF electrode uses a binder to fix the catalyst on the surface of the nickel foam, and the catalyst, binder and nickel foam are squeezed more tightly and firmly by rolling, which can prevent the coating from falling off, making the electrode coating more firm and longer in service life; compared with the self-supporting in-situ growth method and the electrodeposition method, the invention can regulate the loading amount of the FeCoNi-LDH / NF electrode and can have a higher loading amount, which can not only improve the electrochemical performance, but also improve the durability of the electrode for long-term use
[0081] In summary: in the specific implementation, firstly, a mixture of iron salt, cobalt salt and nickel salt is dissolved in deionized water, and stirred and ultrasonically treated to obtain an iron-cobalt-nickel precursor; wherein the mass molar ratio of the iron salt, the cobalt salt and the nickel salt is 1-5:1:1-5; then, a precipitant is added to the iron-cobalt-nickel precursor, and secondary stirring and secondary ultrasonic treatment are performed, wherein the precipitant includes one or more of KOH, NaOH, Na2CO3, NaHCO3, sodium citrate, organic amines, ammonia water or urea; then, an LDH layer control agent is added to obtain a mixed solution; wherein the layer control agent is formamide, dimethylformamide, dimethylacetamide or the like. one or more than two; then add the mixed solution into a hydrothermal reactor; wherein the mass molar ratio of metal ions to precipitants in the mixed solution is 1:0.2-5; then tighten the hydrothermal reactor, and set the hydrothermal reaction temperature and reaction time; wherein the hydrothermal reaction temperature is 80°C-160°C, and the reaction time is 4h-8h; then cool to room temperature, and filter the liquid after the reaction to obtain a precipitate; then wash the precipitate with deionized water and ethanol for multiple times, and dry it to obtain FeCoNi-LDH catalyst powder; then soak the preset nickel foam in HCl, anhydrous ethanol and deionized water, and perform ultrasonic cleaning for multiple times The mixture is washed for 10 minutes each time, and dried for standby use. Then, the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water are mixed and added into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry. The mass molar ratio of the FeCoNi-LDH catalyst powder, the binder, the dispersant, the organic solvent and the deionized water is 10-40: 1-10: 1-5: 45-88. The binder is one or more of AEM membrane solution, PTFE emulsion, PVDF, acrylic resin and carboxymethyl cellulose. The dispersant is metal phosphate, ten One or more of dialkyl sodium sulfate, polyethylene glycol, and polyacrylamide; then the slurry is evenly coated on the preset nickel foam surface, and placed in a drying oven for drying to obtain a FeCoNi-LDH / NF sample; wherein the coating method is one or more of spraying, brushing, comma scraper coating, wire rod coating, and slit extrusion coating, and the drying time of the drying oven is 0.5h-2h; finally, the FeCoNi-LDH / NF sample is rolled by a preset roller press to obtain a FeCoNi-LDH / NF electrode, wherein the roller press pressure is 2t-20t, and the rolling thickness is 0.1mm-0.5mm.
[0082] See attached Figure 1 , is a method for preparing an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis hydrogen production in one embodiment of the present invention, wherein,
[0083] Example 1
[0084] A method for preparing an oxygen evolution catalyst for AEM water electrolysis hydrogen production is prepared according to the following steps:
[0085] S1. Dissolve the mixture containing crystal water Fe(NO3)2, Co(NO3)2, and Ni(NO3)2 in 5L of deionized water according to a set ratio, stir and ultrasonically treat, mix evenly, and obtain an iron-cobalt-nickel precursor;
[0086] S2. Add ammonia water in a set ratio to the iron-cobalt-nickel precursor, perform secondary stirring and secondary ultrasonic treatment, and mix well;
[0087] S3. Add dimethylacetamide in a set ratio;
[0088] S4. The mixed solution is added to a hydrothermal reactor;
[0089] S5. Fasten the hydrothermal reactor, set the hydrothermal reaction temperature to the set temperature, and the reaction time to the set time;
[0090] S6. After the reaction, cool to room temperature and pour out the reaction liquid for filtration;
[0091] S7. The filtered precipitate is washed several times with a mixture of deionized water and ethanol;
[0092] S8. Dry the precipitate to obtain a FeCoNi-LDH catalyst.
[0093] A method for preparing an oxygen evolution electrode for AEM water electrolysis hydrogen production is prepared according to the following steps:
[0094] S1. The nickel foam was immersed in HCl, anhydrous ethanol and deionized water, and ultrasonically cleaned for 10 min each time, and dried for later use;
[0095] S2. Weigh a set ratio of FeCoNi-LDH catalyst powder, AEM membrane solution, polyethylene glycol and solvent, add them to a ball mill, and obtain a uniform slurry by ball milling;
[0096] S3. The slurry was evenly coated on the pretreated nickel foam surface by wire rod coating, placed in an air oven, the reaction temperature was set to 100 ° C, and dried for 1 h;
[0097] S4. The FeCoNi-LDH / NF sample obtained after drying is rolled by a preset roller press to obtain a FeCoNi-LDH / NF electrode.
[0098] The electrochemical performance test was conducted using a Coster CS310M electrochemical workstation. The Coster CS310M electrochemical workstation was used as the test instrument. The test was conducted using a membrane electrode electrolytic cell at room temperature. The electrolytic cell was a two-electrode system. The electrolyte was 1 mol / L KOH. The electrolyte temperature was 60 °C. The scan rate of all linear sweep voltammograms (LSV) was 10 mV·s -1 , the potential scanning range is 1.0V-2.0V.
[0099] Reference Figure 2 , is a scanning electron microscope (SEM) image of the FeCoNi-LDH catalyst prepared in Example 1 of the present invention.
[0100] As can be seen from the figure, the material is in the form of a single-layer sheet. This structure can have more active sites, which is conducive to the oxygen evolution reaction.
[0101] Example 2
[0102] A method for preparing an oxygen evolution catalyst for AEM water electrolysis hydrogen production is prepared according to the following steps:
[0103] S1. A mixture containing Fe(NO3)2, Co(NO3)2 and Ni(NO3)2 containing crystal water is dissolved in 5L of deionized water according to another set ratio, and stirred and ultrasonically treated to mix well to obtain an iron-cobalt-nickel precursor;
[0104] S2. Add ammonia water in a set ratio to the iron-cobalt-nickel precursor, perform secondary stirring and secondary ultrasonic treatment, and mix well;
[0105] S3. Add dimethylacetamide in a set ratio;
[0106] S4. The mixed solution is added to a hydrothermal reactor;
[0107] S5. Fasten the hydrothermal reactor, set the hydrothermal reaction temperature to the set temperature, and the reaction time to the set time;
[0108] S6. After the reaction, cool to room temperature and pour out the reaction liquid for filtration;
[0109] S7. The filtered precipitate is washed several times with a mixture of deionized water and ethanol;
[0110] S8. Dry the precipitate to obtain a FeCoNi-LDH catalyst.
[0111] A method for preparing an oxygen evolution electrode for AEM water electrolysis hydrogen production is prepared according to the following steps:
[0112] S1. The nickel foam was immersed in HCl, anhydrous ethanol and deionized water for ultrasonic cleaning, each cleaning for 10 minutes, and dried for later use;
[0113] S2. Weigh a set ratio of FeCoNi-LDH catalyst powder, AEM membrane solution, polyethylene glycol and solvent, add them to a ball mill, and obtain a uniform slurry by ball milling;
[0114] S3. The slurry was evenly coated on the pretreated nickel foam surface by wire rod coating, placed in an air oven, the reaction temperature was set to 100 ° C, and dried for 1 h;
[0115] S4. The FeCoNi-LDH / NF sample obtained after drying is rolled by a preset roller press to obtain a FeCoNi-LDH / NF electrode.
[0116] The electrochemical performance test was conducted using a Coster CS310M electrochemical workstation. The Coster CS310M electrochemical workstation was used as the test instrument. The test was conducted using a membrane electrode electrolytic cell at room temperature. The electrolytic cell was a two-electrode system. The electrolyte was 1 mol / L KOH. The electrolyte temperature was 60 °C. The scan rate of all linear sweep voltammograms (LSV) was 10 mV·s -1 , the potential scanning range is 1.0V-2.0V.
[0117] That is, the same as Example 1, except that, in the step of preparing the FeCoNi-LDH catalyst, the ratio of Fe(NO3)2, Co(NO3)2, and Ni(NO3)2 nitrates containing crystal water in S1 is adjusted.
[0118] Example 3
[0119] A method for preparing an oxygen evolution catalyst for AEM water electrolysis hydrogen production is prepared according to the following steps:
[0120] S1. The ratio of the mixture containing crystal water Fe(NO3)2, Co(NO3)2, and Ni(NO3)2 was adjusted again, dissolved in 5L of deionized water, stirred and ultrasonically treated, mixed evenly, to obtain an iron-cobalt-nickel precursor;
[0121] S2. Add ammonia water in a set ratio to the iron-cobalt-nickel precursor, perform secondary stirring and secondary ultrasonic treatment, and mix well;
[0122] S3. Add dimethylacetamide in a set ratio;
[0123] S4. The mixed solution is added to a hydrothermal reactor;
[0124] S5. Fasten the hydrothermal reactor, set the hydrothermal reaction temperature to the set temperature, and the reaction time to the set time;
[0125] S6. After the reaction, cool to room temperature and pour out the reaction liquid for filtration;
[0126] S7. The filtered precipitate is washed several times with a mixture of deionized water and ethanol;
[0127] S8. Dry the precipitate to obtain a FeCoNi-LDH catalyst.
[0128] A method for preparing an oxygen evolution electrode for AEM water electrolysis hydrogen production is prepared according to the following steps:
[0129] S1. The nickel foam was immersed in HCl, anhydrous ethanol and deionized water for ultrasonic cleaning, each cleaning for 10 minutes, and dried for later use;
[0130] S2. Weigh a set ratio of FeCoNi-LDH catalyst powder, AEM membrane solution, polyethylene glycol and solvent, add them to a ball mill, and obtain a uniform slurry by ball milling;
[0131] S3. The slurry was evenly coated on the pretreated nickel foam surface by wire rod coating, placed in an air oven, the reaction temperature was set to 100 ° C, and dried for 1 h;
[0132] S4. The FeCoNi-LDH / NF sample obtained after drying is rolled by a preset roller press to obtain a FeCoNi-LDH / NF electrode.
[0133] That is, the same as Example 1, except that, in the step of preparing the FeCoNi-LDH catalyst, the ratio of Fe(NO3)2, Co(NO3)2, and Ni(NO3)2 nitrates containing crystal water in S1 is adjusted.
[0134] Comparative Example 1
[0135] Comparative Example 1: FeCoNi-LDH / NF electrode was prepared by hydrothermal in-situ growth method, and the preparation steps were as follows:
[0136] S1. Prepare 10cm×10cm nickel foam, soak the nickel foam in HCl, anhydrous ethanol and deionized water for ultrasonic cleaning, each cleaning for 10min, and dry it for later use;
[0137] S2. According to the same ratio as in Example 1, the Fe(NO3)2, Co(NO3)2, Ni(NO3)2 mixture was dissolved in 5L deionized water, stirred and ultrasonically treated, and mixed to obtain an iron-cobalt-nickel precursor;
[0138] S3. Add ammonium fluoride and aqueous ammonia to the iron-cobalt-nickel precursor, then add dimethylacetamide, and mix well after secondary stirring and secondary ultrasonic treatment;
[0139] S4. The mixed solution is added to a hydrothermal reactor;
[0140] S5. The nickel foam obtained by pretreatment in S1 is vertically inserted into a hydrothermal reactor and immersed in the solution;
[0141] S6. Fasten the hydrothermal reactor, set the hydrothermal reaction temperature to 80-160°C, and the reaction time to 4h-24h;
[0142] S7. After the reaction is completed, the nickel foam is cooled to room temperature and washed several times with a mixture of deionized water and ethanol;
[0143] S8. Place in an air oven and dry at 100°C for 1 h to obtain a FeCoNi-LDH / NF electrode.
[0144] The electrochemical performance test was performed using an electrochemical workstation, where the electrochemical workstation was a test instrument. The test was performed using a membrane electrode electrolytic cell at room temperature. The electrolytic cell was a two-electrode system, the electrolyte was 1 mol / L KOH, the electrolyte temperature was 60 °C, and the scan rate of all linear sweep voltammograms (LSV) was 10 mV·s -1 , the potential scanning range is 1.0V-2.0V.
[0145] Figure 3 The LSV curves of Example 1, Example 2, Example 3 and Comparative Example 1, i.e., the linear sweep voltammograms, show that the current density of the electrode obtained in Example 1 at a cell voltage of 1.8 V is 715 mA·cm -2 The current density of the electrode obtained in Example 2 at a cell voltage of 1.8 V is 554 mA·cm -2 The current density of the electrode obtained in Example 3 at a cell voltage of 1.8 V is 382 mA·cm -2 The current density of the electrode obtained in Comparative Example 1 at a cell voltage of 1.8 V is 602 mA·cm -2 It can be seen that Example 1 has higher electrochemical performance, and the ratio of the three metals of iron, cobalt and nickel in the FeCoNi-LDH catalyst has a greater influence on the electrochemical performance.
[0146] Figure 4 For Example 1 and Comparative Example 1, the constant current was 800 mA / cm 2By comparing the potential-time curves when the electrode obtained in Example 1 has an overpotential decay amplitude of 0.85 mV / h within 20 h, the overpotential decay amplitude of the electrode obtained in Comparative Example 1 is 2.45 mV / h within 20 h. It can be seen that Example 1 has better stability.
[0147] Compared with the prior art, the prepared FeCoNi-LDH catalyst adopts medium-low temperature liquid phase control, the process is relatively simple, and a product with complete crystal form, uniform particle size distribution and good dispersibility can be obtained without high temperature treatment. The phase is uniform, the purity is high, the crystallization is good, the yield is high, the morphology and size are controllable; the repeatability is high, the electrochemical performance is good, and it can be applied to large-scale industrial production; by changing the reaction temperature, pressure and reaction time, the reaction and crystal growth can be effectively controlled during the hydrothermal process. A single layer of FeCoNi-LDH is prepared, which contains more oxygen evolution active sites, has a larger specific surface area and higher electrocatalytic performance. The prepared FeCoNi-LDH / NF electrode can prevent the coating from falling off, making the electrode coating more firm and longer in life; the loading amount of the FeCoNi-LDH / NF electrode can be regulated, and a higher loading amount can be achieved. A higher loading amount can not only improve the electrochemical performance, but also improve the durability of the electrode for long-term use.
[0148] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A method for preparing an oxygen evolution catalyst and an oxygen evolution electrode for AEM water electrolysis hydrogen production, It is characterized in that include: S1, dissolving a mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating the mixture to obtain an iron-cobalt-nickel precursor; S2, adding a precipitant to the iron-cobalt-nickel precursor, performing secondary stirring and secondary ultrasonic treatment, wherein the precipitant includes KOH, NaOH, Na 2 CO 3 、NaHCO 3 , sodium citrate, organic amines, ammonia water or urea, one or more thereof; S3, adding an LDH layer control agent to obtain a mixed solution; wherein the layer control agent is one or more of formamide, dimethylformamide, and dimethylacetamide; S4, adding the mixed solution into a hydrothermal reaction kettle; S5, tightening the hydrothermal reactor and setting the hydrothermal reaction temperature and reaction time; S6, cooling to room temperature, and filtering the liquid after the reaction to obtain a precipitate; S7, washing and drying the precipitate to obtain FeCoNi-LDH catalyst powder; S8, mixing the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them to a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry; S9, evenly coating the slurry on a preset nickel foam surface, and placing it in a drying oven for drying to obtain a FeCoNi-LDH / NF sample; S10, rolling the FeCoNi-LDH / NF sample by a preset rolling press to obtain a FeCoNi-LDH / NF electrode.
2. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of dissolving the mixture of iron salt, cobalt salt and nickel salt in deionized water, stirring and ultrasonically treating the mixture to obtain the iron-cobalt-nickel precursor further includes: The mass molar ratio of the iron salt, the cobalt salt and the nickel salt is 1-5:1:1-5.
3. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of adding the mixed solution into the hydrothermal reaction kettle further comprises: The mass molar ratio of metal ions to precipitants in the mixed solution is 1:0.2-5.
4. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of fastening the hydrothermal reactor and setting the hydrothermal reaction temperature and reaction time also includes: The hydrothermal reaction temperature is 80°C-160°C, and the reaction time is 4h-8h.
5. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of washing and drying the precipitate to obtain FeCoNi-LDH catalyst powder also includes: The precipitate was washed several times with deionized water and ethanol.
6. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that Before the step of mixing the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry, the step further comprises: The preset nickel foam was immersed in HCl, anhydrous ethanol and deionized water respectively, ultrasonically cleaned for multiple times, and dried.
7. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 6, It is characterized in that The step of immersing the preset nickel foam in HCl, anhydrous ethanol and deionized water respectively, performing ultrasonic cleaning multiple times, and drying also includes: Each cleaning time is 10 minutes.
8. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of mixing the FeCoNi-LDH catalyst powder, binder, dispersant, organic solvent and deionized water and adding them into a planetary mixer, a ball mill, a deaerator or a high-speed disperser for stirring to obtain a slurry also includes: The mass molar ratio of the FeCoNi-LDH catalyst powder, the binder, the dispersant and the organic solvent or the deionized water is 10-40:1-10:1-5:45-88, wherein the binder is one or more of AEM membrane solution, PTFE emulsion, PVDF, acrylic resin, and carboxymethyl cellulose; and the dispersant is one or more of metal phosphate, sodium dodecyl sulfate, polyethylene glycol, and polyacrylamide.
9. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of uniformly coating the slurry on a preset nickel foam surface and placing the slurry in a drying oven for drying further includes: The coating method is one or more of spray coating, brush coating, comma blade coating, wire rod coating, and slit extrusion coating; The drying time of the drying box is 0.5h-2h.
10. The method for preparing the oxygen evolution catalyst and oxygen evolution electrode for AEM water electrolysis hydrogen production according to claim 1, It is characterized in that The step of rolling the FeCoNi-LDH / NF sample by a roller press to obtain a FeCoNi-LDH / NF electrode comprises: The roller press pressure is 2t-20t, and the roller pressing thickness is 0.1mm-0.5mm.
Citation Information
Patent Citations
A foamed nickel-supported iron-cobalt-nickel metal nanocatalyst, its preparation method and application
CN111495417B
NiFeCo-LDH / NF electrocatalyst and preparation method thereof
CN114892207A
Iron-cobalt-nickel double hydroxide nanocage electro-catalysis oxygen evolution material and preparation method thereof
CN115386908A
Cited By
Iron-cobalt-nickel-chromium oxide nano material as well as preparation method and application thereof
CN119877001A
Preparation method and application of ultrathin ferronickel layered double hydroxide
CN120817638A
Preparation method and application of ultrathin nickel-iron layered double hydroxide