Ultrahigh-conductivity cold-rammed steel bar paste as well as preparation method and application thereof
By using iron particles and binders of specific mass and particle sizes to prepare ultra-high conductive cold pounding steel rod paste, the problem of reducing the voltage drop of the electrolytic cell is solved, and the production efficiency and energy consumption of aluminum electrolytics are improved.
Patent Information
- Application Number
- CN202410977379.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has problems of complex operation and high cost in reducing the voltage drop of the electrolytic cell, making it difficult to effectively improve the production efficiency of aluminum electrolytics and reduce energy consumption.
Ultra-high conductive cold pounding steel rod paste is prepared using iron particles of specific mass and particle sizes, and a low resistivity material is formed by preheating and stirring, and used in aluminum electrolytic cells to significantly reduce the pressure drop at the bottom of the tank.
It realizes a reduction in the voltage drop of the electrolytic cell with simple operation and low cost, improves the production efficiency and current efficiency of aluminum electrolytics, and reduces the power consumption.
Smart Images

Figure BDA0004957267970000081 
Figure BDA0004957267970000091
Abstract
Description
Technical Field
[0001] The invention relates to an ultra-high conductive cold-rammed steel rod paste and a preparation method and application thereof, belonging to the technical field of electrolytic aluminum. Background Art
[0002] The voltage drop of the electrolytic cell refers to the resistance drop caused by the electrolyte concentration, cell span, cell wall, anode and cathode, etc. due to the influence of various electrical, thermal and fluid factors in the electrolytic cell. The voltage drop of the electrolytic cell has a great impact on the production efficiency and energy consumption of aluminum electrolysis. A higher voltage drop of the electrolytic cell will lead to excessive electrolyte concentration, increase the generation of anode bubbles, increase the resistance drop, thereby reducing the current efficiency and aluminum production efficiency, and consume a lot of electricity, increasing production costs.
[0003] At present, in order to reduce the pressure drop at the bottom of the electrolytic cell, methods such as improving the electrolytic cell structure and optimizing the electrolysis process are usually adopted. However, these methods have problems such as high transformation cost and complex operation.
[0004] Exploring a method to reduce the pressure drop of the electrolytic cell while being simple to operate has become a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention
[0005] The invention provides an ultra-high conductive cold-rammed steel rod paste, which comprises iron particles of specific mass parts and specific particle sizes and a binder. When used in an electrolytic cell, the ultra-high conductive cold-rammed steel rod paste can significantly reduce the pressure drop of the electrolytic cell and improve the production efficiency of aluminum electrolysis.
[0006] The invention provides a method for preparing ultra-high conductive cold-rammed steel rod paste. The method is simple, easy to operate, and has low production cost, and can prepare the ultra-high conductive cold-rammed steel rod paste.
[0007] The present invention also provides an aluminum electrolysis cell, which comprises the ultra-high conductive cold-rammed steel rod paste and has a lower cell bottom pressure drop.
[0008] On one hand, the present invention provides an ultra-high conductive cold-rammed steel rod paste, which comprises, by weight, 10-30 parts of first iron particles, 20-40 parts of second iron particles, 20-40 parts of third iron particles, and 10-30 parts of a binder;
[0009] The particle size of the first iron particles is 1-2 mm, the particle size of the second iron particles is 0.15-1 mm, and the particle size of the third iron particles is not higher than 0.75 mm.
[0010] The ultrahigh conductive cold-rammed steel rod paste as described above comprises, by mass, 10-20 parts of the first iron particles, 20-30 parts of the second iron particles, 30-40 parts of the third iron particles, and 10-20 parts of the binder.
[0011] In the ultra-high conductive cold-rammed steel rod paste as described above, the particle size of the first iron particles is 1.5-2 mm.
[0012] In the ultra-high conductive cold-rammed steel rod paste as described above, the particle size of the second iron particles is 0.75-1 mm.
[0013] In the ultra-high conductive cold-rammed steel rod paste as described above, the particle size of the third iron particles is not greater than 0.15 mm.
[0014] The ultra-high conductive cold-rammed steel rod paste as described above, wherein the binder is phenolic resin.
[0015] In another aspect, the present invention provides a method for preparing the ultra-high conductive cold-rammed steel rod paste as described above, comprising the following steps:
[0016] 1) weighing first iron particles, second iron particles, and third iron particles, performing preheating treatment, and then stirring to obtain a first mixture;
[0017] 2) Adding a binder to the first mixture and stirring the mixture to obtain the ultra-high conductive cold-rammed steel rod paste.
[0018] In the preparation method as described above, the temperature of the preheating treatment is 20-60° C. and the time is 15-25 min.
[0019] In the preparation method as described above, in step 2), the stirring temperature is 50-60°C.
[0020] In another aspect, the present invention provides an aluminum electrolytic cell, comprising the ultra-high conductive cold-rammed steel rod paste as described above or the ultra-high conductive cold-rammed steel rod paste prepared by the preparation method as described above.
[0021] The ultrahigh conductive cold-rammed steel rod paste provided by the present invention comprises iron particles and a binder of specific mass parts and specific particle sizes. With the combination of iron particles and binders of different particle sizes, the resistivity is lower than 2μΩ·m, which can significantly reduce the voltage drop at the bottom of the tank and improve the electrolysis efficiency.
[0022] The method for preparing the ultra-high conductive cold-rammed steel rod paste provided by the present invention can prepare the ultra-high conductive cold-rammed steel rod paste, which can significantly reduce the bottom pressure drop of the electrolytic cell when used in the electrolytic cell.
[0023] The aluminum electrolytic cell provided by the present invention comprises the ultra-high conductive cold-rammed steel rod paste and has a lower pressure drop at the bottom of the cell. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] On the one hand, the present invention provides an ultra-high conductive cold-rammed steel rod paste, which includes 10-30 parts by mass of first iron particles, 20-40 parts by mass of second iron particles, 20-40 parts by mass of third iron particles, and 10-30 parts by mass of a binder; wherein the particle size of the first iron particles is 1-2 mm, the particle size of the second iron particles is 0.15-1 mm, and the particle size of the third iron particles is not higher than 0.75 mm.
[0026] Specifically, the first iron particles, the second iron particles, and the third iron particles in the present invention are pure iron particles, which can be purchased from the market.
[0027] The ultra-high conductive cold-rammed steel rod paste of the present invention refers to a cold-rammed steel rod paste with a room temperature resistivity of no more than 2 μΩ·m.
[0028] Wherein the mass fraction of the first iron particles is 10-30 parts, for example, the mass fraction of the first iron particles includes but is not limited to 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts or any range between two of them. The mass fraction of the second iron particles includes but is not limited to 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts or any range between two of them. The mass fraction of the third iron particles includes but is not limited to 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 40 parts or any range between two of them.
[0029] In the present invention, the particle sizes of the first iron particles, the second iron particles, and the third iron particles refer to the particle sizes of all iron particles. For example, if the particle size of the first iron particles is 1-2 mm, then the particle size of the smallest particle in the first iron particles should not be less than 1 mm, and the particle size of the largest particle should not be higher than 2 mm.
[0030] The invention uses iron particles as aggregates for cold ramming paste, which have good thermal conductivity, mechanical properties, economy and processability.
[0031] When the ultra-high conductive cold-rammed steel rod paste provided by the present invention is used in an aluminum electrolytic cell, it can significantly reduce the bottom voltage drop of the electrolytic cell and improve the electrolysis efficiency. The inventors believe that the reason may be that the material itself is upgraded from carbon material to metal material, and the conductive performance is significantly improved, thereby reducing the bottom voltage drop of the electrolytic cell.
[0032] Furthermore, in a specific embodiment of the present invention, the first iron particles are included in an amount of 10-20 parts, the second iron particles are included in an amount of 20-30 parts, the third iron particles are included in an amount of 30-40 parts, and the binder is included in an amount of 10-20 parts by mass.
[0033] In detail, in parts by mass, the first iron particles include but are not limited to 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts or a range between any two of them, the second iron particles include but are not limited to 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts or a range between any two of them, the third iron particles include but are not limited to 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts or a range between any two of them, and the binder includes but is not limited to 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts or a range between any two of them.
[0034] When the ultra-high conductive cold-rammed steel rod paste includes the above-mentioned mass parts of the first iron particles, the second iron particles and the third iron particles, it can not only enhance the conductive properties and mechanical strength of the paste and improve the uniformity of the material, but also better realize the synergistic effect between iron particles of different particle sizes, thereby further reducing the pressure drop at the bottom of the slot.
[0035] Furthermore, in a specific embodiment of the present invention, the particle size of the first iron particles is 1.5-2 mm.
[0036] In detail, the particle size of the first iron particles includes but is not limited to 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2.0 mm or a range between any two thereof.
[0037] In one specific embodiment, the particle size of the first iron particles is 2 mm.
[0038] Furthermore, in a specific embodiment of the present invention, the particle size of the second iron particles is 0.75-1 mm.
[0039] Specifically, the particle size of the second iron particles includes, but is not limited to, 0.75 mm, 0.80 mm, 0.85 mm, 0.9 mm, 0.95 mm, 1.0 mm, or a range between any two thereof.
[0040] In one specific embodiment, the particle size of the second iron particles is 1 mm.
[0041] Furthermore, in a specific embodiment of the present invention, the particle size of the third iron particles is not greater than 0.15 mm.
[0042] In one specific embodiment, the particle size of the third iron particles is 10-45 μm.
[0043] When the particle size of the iron particles is within the above range, the bulk density of the product is most suitable and the synergistic effect between the various types of iron particles is best.
[0044] Furthermore, in a specific embodiment of the present invention, the binder is a phenolic resin.
[0045] The binder in the ultra-high conductive cold-rammed steel rod paste can not only play the role of bonding and curing, but also can adjust the rheological properties of the paste, enhance the mechanical strength, and improve the stability and durability of the cold-rammed steel rod paste.
[0046] In another aspect, the present invention provides a method for preparing the ultra-high conductive cold-rammed steel rod paste as described above, comprising the following steps:
[0047] 1) weighing first iron particles, second iron particles, and third iron particles, performing preheating treatment, and then stirring to obtain a first mixture;
[0048] 2) Adding a binder to the first mixture and stirring the mixture to obtain an ultra-high conductive cold-rammed steel rod paste.
[0049] Specifically, in step 1), first iron particles with a particle size of 1.5-2 mm, second iron particles with a particle size of 0.15-1 mm, and third iron particles with a particle size not higher than 0.15 mm are weighed according to a certain mass ratio, the three are preheated, then stirred, and mixed evenly to obtain a first mixture.
[0050] In step 2), a binder is added to the first mixture, followed by stirring to obtain an ultra-high conductive cold-rammed steel rod paste.
[0051] It can be understood that the stirring process can be performed using a stirring device. The present invention does not limit the specific type of the stirring device, and a stirring device commonly used in the art can be selected.
[0052] The present invention does not limit the stirring time, as long as the iron particles of different particle sizes can be evenly mixed. In a specific embodiment, the stirring time is 20-40 minutes.
[0053] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided by the present invention has simple process, is easy to operate and has low production cost. The ultra-high conductive cold-rammed steel rod paste prepared according to the preparation method can significantly reduce the bottom pressure drop of the aluminum electrolytic cell and improve the electrolysis efficiency when used in the aluminum electrolytic cell.
[0054] Furthermore, in a specific embodiment of the present invention, the temperature of the preheating treatment is 20-60° C., and the time is 15-25 min.
[0055] In detail, the temperature of the preheat treatment includes but is not limited to 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 60°C or a range between any two of them, and the time of the preheat treatment includes but is not limited to 15min, 18min, 20min, 22min, 24min, 25min or a range between any two of them.
[0056] When the temperature and time of the preheating treatment are within the above range, the adhesive can fully contact the metal material and the wetting effect is optimal. When it exceeds the control range, the adhesive ages and the final effect of the product is poor.
[0057] Furthermore, in a specific embodiment of the present invention, in step 2), the stirring temperature is 50-60°C.
[0058] In detail, the temperature of the stirring treatment includes but is not limited to 50°C, 51°C, 52°C, 53°C, 54°C, 55°C, 56°C, 57°C, 58°C, 59°C, 60°C or a range between any two of them.
[0059] When the stirring temperature is within the above range, the phenolic resin achieves the maximum wetting effect.
[0060] In another aspect, the present invention provides an aluminum electrolytic cell, comprising the ultra-high conductive cold-rammed steel rod paste as described above or the ultra-high conductive cold-rammed steel rod paste prepared by the preparation method as described above.
[0061] Ultra-high conductive cold-rammed steel rod paste is mainly used for the maintenance and repair of aluminum electrolytic cells to ensure that the aluminum electrolytic cells can carry out aluminum electrolysis production stably and efficiently.
[0062] It can be understood that the aluminum electrolysis cell also includes an electrolysis cell shell, a cathode, an anode, an electrolysis cell top cover and accessories, and a power supply system.
[0063] The present invention does not limit the specific types or parameters of the electrolytic cell shell, cathode, anode, electrolytic cell top cover and accessories and power supply system in the aluminum electrolytic cell, and the device types and parameters commonly used in the field can be selected.
[0064] Hereinafter, the ultrahigh conductive cold-rammed steel rod paste provided by the present invention will be introduced in detail through specific embodiments.
[0065] Example 1
[0066] The method for preparing the ultra-high conductive cold-rammed steel rod paste provided in this embodiment comprises the following steps:
[0067] 1) Weigh 20 g of first iron particles with a particle size of 2 mm, 30 g of second iron particles with a particle size of 1 mm, and 30 g of third iron particles with a particle size of 0.75 mm, preheat them at 40° C. for 50 min, and then stir them to obtain a first mixture;
[0068] 2) Add 20 g of a binder to the first mixture and stir the mixture at 50° C. to obtain an ultra-high conductive cold-rammed steel rod paste.
[0069] Example 2
[0070] The method for preparing the ultra-high conductive cold-rammed steel rod paste provided in this embodiment comprises the following steps:
[0071] 1) Weigh 10 g of first iron particles with a particle size of 1.5 mm, 40 g of second iron particles with a particle size of 0.15 mm, and 40 g of third iron particles with a particle size of 0.15 mm, preheat them at 20° C. for 25 min, and then stir them to obtain a first mixture;
[0072] 2) Add 10 g of a binder to the first mixture and stir the mixture at 60° C. to obtain an ultra-high conductive cold-rammed steel rod paste.
[0073] Example 3
[0074] The method for preparing the ultra-high conductive cold-rammed steel rod paste provided in this embodiment comprises the following steps:
[0075] 1) Weigh 30 g of first iron particles with a particle size of 1.8 mm, 20 g of second iron particles with a particle size of 0.5 mm, and 20 g of third iron particles with a particle size of 44 μm, preheat them at 60° C. for 15 min, and then stir them to obtain a first mixture;
[0076] 2) Add 30 g of a binder to the first mixture and stir the mixture at 55° C. to obtain an ultra-high conductive cold-rammed steel rod paste.
[0077] Example 4
[0078] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this embodiment is basically the same as that in Example 1, except that:
[0079] The first iron particles weigh 30 g, the second iron particles weigh 35 g, the third iron particles weigh 20 g, and the binder weighs 25 g.
[0080] Example 5
[0081] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this embodiment is basically the same as that in Example 1, except that:
[0082] The particle size of the first iron particles is 1 mm.
[0083] Example 6
[0084] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this embodiment is basically the same as that in Example 1, except that:
[0085] The particle size of the second iron particles is 0.5 mm.
[0086] Example 7
[0087] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this embodiment is basically the same as that in Example 1, except that:
[0088] The particle size of the third iron particles is 0.35 μm.
[0089] Example 8
[0090] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this embodiment is basically the same as that in Example 1, except that:
[0091] In step 1), the preheating temperature is 65° C. and the time is 30 min.
[0092] Example 9
[0093] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this embodiment is basically the same as that in Example 1, except that:
[0094] In step 2), the stirring temperature is 45°C.
[0095] Comparative Example 1
[0096] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this comparative example is basically the same as that in Example 1, except that:
[0097] The first iron particles weigh 35 g, the second iron particles weigh 15 g, the third iron particles weigh 15 g, and the binder weighs 35 g.
[0098] Comparative Example 2
[0099] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this comparative example is basically the same as that in Example 1, except that:
[0100] The particle size of the first iron particles is 2.5 mm, the particle size of the second iron particles is 1.5 mm, and the particle size of the third iron particles is 0.55 mm.
[0101] Comparative Example 3
[0102] The preparation method of the ultra-high conductive cold-rammed steel rod paste provided in this comparative example is basically the same as that in Example 1, except that:
[0103] The first iron particles, the second iron particles, and the third iron particles are all replaced with carbon materials.
[0104] Test Case
[0105] The ultra-high conductive cold-rammed steel rod paste provided in all the embodiments and comparative examples was applied to an aluminum electrolytic cell and the bottom voltage drop of the cell was tested, specifically including:
[0106] The room temperature resistivity was tested and compared using the cold ramming paste test standard YS / T 63.2-2006.
[0107] Table 1
[0108]
[0109]
[0110] It can be seen from Table 1 that the room temperature resistivity of the superconducting cold-rammed steel rod paste provided in the present application is less than 2 μΩ·m, which can significantly reduce the voltage drop at the bottom of the slot.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. An ultra-high conductive cold-rammed steel rod paste, characterized in that: The invention comprises, by weight, 10-30 parts of first iron particles, 20-40 parts of second iron particles, 20-40 parts of third iron particles, and 10-30 parts of a binder; The particle size of the first iron particles is 1-2 mm, the particle size of the second iron particles is 0.15-1 mm, and the particle size of the third iron particles is not higher than 0.75 mm.
2. The ultra-high conductive cold-rammed steel rod paste according to claim 1, characterized in that: In parts by mass, the composition comprises 10-20 parts of the first iron particles, 20-30 parts of the second iron particles, 30-40 parts of the third iron particles, and 10-20 parts of the binder.
3. The ultra-high conductive cold-rammed steel rod paste according to claim 1 or 2, characterized in that: The particle size of the first iron particles is 1.5-2 mm.
4. The ultra-high conductive cold-rammed steel rod paste according to any one of claims 1 to 3, characterized in that: The particle size of the second iron particles is 0.75-1 mm.
5. The ultra-high conductive cold-rammed steel rod paste according to any one of claims 1 to 4, characterized in that: The particle size of the third iron particles is not greater than 0.15 mm.
6. The ultra-high conductive cold-rammed steel rod paste according to any one of claims 1 to 5, characterized in that: The binder is phenolic resin.
7. A method for preparing the ultra-high conductive cold-rammed steel rod paste according to any one of claims 1 to 6, characterized in that: The following steps are involved: 1) weighing first iron particles, second iron particles, and third iron particles, performing preheating treatment, and then stirring to obtain a first mixture; 2) Adding a binder to the first mixture and stirring the mixture to obtain the ultra-high conductive cold-rammed steel rod paste.
8. The preparation method according to claim 7, characterized in that: The preheating treatment is performed at a temperature of 20-60° C. and for a time of 15-25 minutes.
9. The preparation method according to claim 7 or 8, characterized in that: In step 2), the stirring temperature is 50-60°C.
10. An aluminum electrolysis cell, characterized in that: The invention comprises the ultra-high conductive cold-rammed steel rod paste described in any one of claims 1 to 6 or the ultra-high conductive cold-rammed steel rod paste prepared by the preparation method described in any one of claims 7 to 9.