Composite copper foil preparation system and preparation method thereof
By using unwinding and winding mechanisms to press the copper foil onto the polymer film in the preparation of composite copper foil, the problems of high equipment investment and low production efficiency of vacuum coating method are solved, and the preparation of composite copper is achieved at low cost and rapid Foil improves the toughness and conductivity of copper foil.
Patent Information
- Application Number
- CN202411093425.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing composite copper foil preparation technology, the vacuum coating method equipment has high investment, strict process requirements and low production efficiency, resulting in limited application of composite copper foil.
The unwinding mechanism and the winding mechanism are used to collect and unwind the polymer film. The copper foil electrolytic deposition line deposits the copper foil onto the deposition roller. The copper foil is pressed onto the polymer film by rotating the deposition roller and peeling it to form composite copper. Foil simplifies the process flow and improves production efficiency.
The vacuum coating method has overcome the problems of large investment in equipment, strict process requirements and low production efficiency, and has achieved low cost and rapid preparation of composite copper foil, which has reduced the amount of metal copper, and improved the strength and conductivity of copper foil.
Smart Images

Figure CN118932440A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite copper foil production, and in particular to a composite copper foil preparation system and a preparation method thereof. Background Art
[0002] As a key material in the fields of copper-clad laminates for printed circuit boards and current collectors for energy storage batteries, the demand for electrolytic copper foil continues to rise with the continuous development of the electronics industry and energy storage batteries. On the other hand, it has become an urgent desire for copper foil application companies to continuously reduce the price and weight of the copper foil used. For example, if the copper foil used as the current collector of lithium batteries is reduced by half with the same area, not only can the price be greatly reduced, but the technical indicators such as the energy storage density per unit weight of lithium batteries will also be greatly improved.
[0003] In order to achieve this goal, the current mainstream technical solution is to use composite copper foil instead of electrolytic copper foil. The composite copper foil is formed by combining polymer film material and copper film, in which the thickness of the copper film is only about 1 micron. For pure electrolytic copper foil, the existing technical conditions and the requirements for copper foil strength require at least 4.5 microns.
[0004] Because polymer film materials are insulating materials, composite copper foil cannot be formed directly on them through electrodeposition. The current mainstream technical route is to first use vacuum coating to deposit a layer of nano-copper film on the polymer film material, and then use electrolysis to further deposit the copper film to achieve the required thickness. There are also reports on technologies that directly use vacuum coating to deposit the required copper film thickness in one go, without the need for electrolytic deposition to prepare composite copper films.
[0005] However, on the one hand, when the vacuum coating method is used to prepare copper films, the equipment manufacturing required is very technically demanding and expensive. The vacuum coating process is strict and has not yet been sufficiently verified and guaranteed for mass production. On the other hand, during the vacuum coating process, there is a huge energy output in the coating space, which can easily cause the polymer film material to overheat and deform, resulting in coating failure. To ensure the yield, it is necessary to use relatively more expensive and heat-resistant polymer film materials while strictly controlling the heat, which undoubtedly seriously reduces the advantages of the composite copper foil. Summary of the invention
[0006] In view of the above problems, the purpose of the present invention is to provide a composite copper foil preparation system and preparation method thereof, in which a polymer film is unwound and reeled by an unwinding mechanism and a reeling mechanism, and a copper foil electrolytic deposition line deposits the copper foil onto a deposition roller, and the deposition roller transfers and presses the copper foil onto the polymer film during rotation, and the polymer film peels the copper foil off the deposition roller to form a composite copper foil, thereby overcoming the current mainstream method of preparing composite copper foil based on vacuum coating, which has the disadvantages of large equipment investment, strict process requirements, and low production efficiency, which restrict the rapid development and application of composite copper foil.
[0007] The technical solution adopted by the present invention is as follows:
[0008] A composite copper foil preparation system comprises at least two deposition rollers arranged opposite to each other, each of the deposition rollers is connected to a copper foil electrolytic deposition line, an unwinding mechanism and a rewinding mechanism are respectively arranged on both sides of the deposition roller, and a polymer film passing through a gap between the two deposition rollers is wound around the unwinding mechanism and the rewinding mechanism.
[0009] Preferably, a tension adjustment mechanism for adjusting the tension of the polymer film is provided between the unwinding mechanism and the rewinding mechanism.
[0010] Preferably, the two deposition rollers are connected with an adjustment base capable of adjusting the gap between the two deposition rollers.
[0011] Preferably, the unwinding mechanism is provided with a glue coating device for coating the surface of the polymer film with glue.
[0012] A composite copper foil preparation method, using the composite copper foil preparation system, the preparation method comprises the following steps:
[0013] S1. Place the rolled polymer film on the unwinding mechanism, unwind the polymer film and pull the polymer film through the gap between the two deposition rollers, then wind the polymer film on the winding mechanism, adjust the tension adjustment mechanism to ensure that the polymer film moves evenly and without deviation, and prepare and fix the walking speed;
[0014] S2. Preparation work for the copper foil electrolytic deposition line, including preparation for electrolyte filtration and concentration adjustment, preparation for anode electrolytic copper plate, preparation for deposition roller and preparation for electrolytic deposition power supply. The power supply power is set according to the effective deposition area and rotation speed of the deposition roller to control the deposition rate;
[0015] S3. Check the contact pressure between the deposition roller and the polymer film to ensure that there is sufficient pressing force between the copper foil on the deposition roller and the polymer film, so that the bonding force between the copper foil and the polymer film is greater than the bonding force of the copper foil on the deposition roller;
[0016] S4. After the preparation and inspection are completed, the unwinding mechanism and the rewinding mechanism are started to rewind and unwind, and the copper foil electrolytic deposition line works in sequence. The copper foil is deposited on the deposition roller and transferred and pressed onto the polymer film. The polymer film peels the copper foil off the deposition roller to form a composite copper foil.
[0017] S5. When a composite copper foil roll is prepared, the copper foil electrolytic deposition line, the unwinding mechanism and the rewinding mechanism are stopped in sequence, thus completing a process.
[0018] Preferably, the walking speed is 0.01-100 m / min.
[0019] Preferably, the deposition rate is 0.01-100 μm / min.
[0020] Preferably, the bonding force between the copper foil and the polymer film is twice or more than the bonding force of the copper foil on the deposition roller.
[0021] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0022] The polymer film is unwound and rolled up by the unwinding mechanism and the rewinding mechanism, and the copper foil electrolytic deposition line deposits the copper foil onto the deposition roller. The deposition roller transfers and presses the copper foil onto the polymer film during rotation, and the polymer film peels the copper foil off the deposition roller to form a composite copper foil. In the lithium battery industry, the use of composite copper foil to replace traditional electrolytic copper foil has important functions such as greatly reducing the battery's deadweight and improving the toughness of the battery collector without reducing the conductive performance. The current mainstream method of preparing composite copper foil based on vacuum coating has unfavorable factors that restrict the rapid development and application of composite copper foil, such as large equipment investment, strict process requirements, and low production efficiency. The present invention has greatly overcome these problems. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 A schematic diagram of a system provided by an embodiment of the present invention;
[0025] Description of the drawings: 1-copper foil electrolytic deposition line; 2-deposition roller; 3-polymer film; 4-winding mechanism; 5-unwinding mechanism. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.
[0027] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In the description of the present invention, it should be noted that if the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside" and the like appear, the orientation or position relationship indicated is based on the orientation or position relationship shown in the accompanying drawings, or is the orientation or position relationship in which the product of the application is usually placed when used. It is only for the convenience of describing the present invention and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0029] Combine the following Figure 1 The present invention is described in detail.
[0030] Example
[0031] A composite copper foil preparation system comprises at least two deposition rollers 2 arranged opposite to each other, each deposition roller 2 is connected to a copper foil electrolytic deposition line 1, an unwinding mechanism 5 and a rewinding mechanism 4 are respectively arranged on both sides of the deposition roller 2, and a polymer film 3 passing through the gap between the two deposition rollers 2 is wound around the unwinding mechanism 5 and the rewinding mechanism 4.
[0032] The copper foil electrolytic deposition line 1 includes a deposition power supply, an electrolytic cell, a copper dissolving plate and an electrolyte filter (all of which are prior arts). The copper foil electrolytic deposition line 1 deposits the copper foil on the surface of a deposition roller 2 by electrolysis. At the same time, the deposition roller 2 is continuously rotating to uniformly press the copper foil onto the polymer film 3. Driven by an unwinding mechanism 5 and a winding mechanism 4 (both of which are prior arts), the polymer film 3 can continuously and uniformly peel off the copper foil on the surface of the deposition roller 2. The operation is simple and the production efficiency is high.
[0033] One of the two deposition rollers 2 can be selected to deposit copper foil, and the other one can be selected not to deposit copper foil, so as to achieve single-sided copper foil attachment of the polymer film 3. Four deposition rollers 2 can also be used for production, specifically: two deposition rollers 2 are arranged opposite to each other as a group, one deposition roller 2 is used for deposition, and the other deposition roller 2 is not used for deposition (i.e., a laminating roller), one group of deposition rollers 2 only laminates copper foil on one side of the polymer film 3, and the other group of deposition rollers 2 laminates copper foil on the other side of the polymer film 3, but this arrangement requires two more laminating rollers, and the production cost is relatively high, so it is preferred to use two deposition rollers 2 to laminate copper foil at the same time.
[0034] A tension adjusting mechanism (the tension adjusting mechanism is a prior art) for adjusting the tension of the polymer film 3 is arranged between the unwinding mechanism 5 and the winding mechanism 4 to ensure that the polymer film 3 moves uniformly and without deviation, and to prepare and fix the walking speed; the tension adjusting mechanism includes a mounting seat movable in a direction perpendicular to the plane where the polymer film 3 is located, and a rotating roller that rolls in contact with the polymer film 3 is rotatably arranged on the mounting seat. By adjusting the distance between the mounting seat and the polymer film 3, the force of the rotating roller abutting against the surface of the polymer film 3 is changed, thereby adjusting the tension of the polymer film 3.
[0035] The two deposition rollers 2 are connected with an adjustment base (the adjustment base is prior art) that can adjust the gap between the two deposition rollers 2. The deposition rollers 2 can adjust the gap between the two deposition rollers 2 through the adjustment base, thereby adapting to the production of polymer films 3 with different thicknesses.
[0036] The unwinding mechanism 5 is provided with a glue coating device (the glue coating device is a prior art) for coating the surface of the polymer film 3. The glue coating device can improve the adhesion of the polymer film 3, thereby better peeling the electrolytic copper foil from the deposition roller 2.
[0037] A composite copper foil preparation method, using a composite copper foil preparation system, the preparation method comprises the following steps:
[0038] S1, put the rolled polymer film 3 on the unwinding mechanism 5, unwind the polymer film 3 and pull the polymer film 3 through the gap between the two deposition rollers 2, then wind the polymer film 3 on the winding mechanism 4, adjust the tension adjustment mechanism to ensure that the polymer film 3 moves evenly and without deviation, and prepare and fix the walking speed;
[0039] S2, the copper foil electrolytic deposition line 1 performs preparation work, including preparation for electrolyte filtration and concentration adjustment, preparation for anode electrolytic copper plate, preparation for deposition roller 2 and preparation for electrolytic deposition power supply. The power supply power is set according to the effective deposition area of deposition roller 2 and the rotation speed of deposition roller 2, so as to control the deposition rate;
[0040] S3, check the contact pressure between the deposition roller 2 and the polymer film 3 to ensure that there is sufficient pressing force between the copper foil on the deposition roller 2 and the polymer film 3, so that the bonding force between the copper foil and the polymer film 3 is greater than the bonding force of the copper foil on the deposition roller 2;
[0041] S4, after the preparation and inspection are completed, the unwinding mechanism 5 and the rewinding mechanism 4 are started to rewind and unwind, and the copper foil electrolytic deposition line 1 works in sequence, the copper foil is deposited on the deposition roller 2 and transferred and pressed onto the polymer film 3, and the polymer film 3 peels the copper foil off the deposition roller 2 to form a composite copper foil;
[0042] S5. When a composite copper foil roll is prepared, the copper foil electrolytic deposition line 1, the unwinding mechanism 5 and the rewinding mechanism 4 are stopped in sequence, and a process is completed.
[0043] The travel speed is 0.01-100 m / min, and the deposition speed is 0.01-100 μm / min. The travel speed of the polymer film 3 and the deposition speed of the copper foil are properly adjusted so that the copper foil can be evenly pressed onto the polymer film 3 .
[0044] The bonding force between the copper foil and the polymer film 3 is twice or more than the bonding force of the copper foil on the deposition roller 2. For example, the bonding force between the copper foil and the polymer film 3 is 1-1000 N / cm 2 , the bonding force of the copper foil on the deposition roller 2 is 0.1-100N / cm 2 , to ensure that the polymer film 3 can be smoothly peeled off the copper foil and form a composite copper foil.
[0045] Specific implementation process:
[0046] A deposition roller 2 with a diameter of 2 m and a height (the width of the resulting copper foil) of 1 m and two copper foil electrolytic deposition lines 1 are used, and the deposition rollers 2 at the terminals are arranged in parallel and in contact with each other with a gap of 0.1-10 microns.
[0047] The contact height between the solution in the electrolytic cell and the deposition roller 2 is 0-50 cm, generally not exceeding 30 cm, to ensure that there is enough space for the unfolded polymer film 3 to pass through the gap between the two deposition rollers 2 .
[0048] The two deposition rollers 2 rotate in a circle relative to each other to ensure that the polymer film 3 passing through the mutual extrusion zone moves in one direction, for example, the lower side is unwinding and the upper side is winding.
[0049] The polymer film 3 can be a PE film with a length of 1000 meters, which is hung on the unwinding mechanism 5. Initially, the polymer film 3 is manually drawn out, passes through the extrusion area of the deposition roller 2, and is wrapped on the winding mechanism 4, completing the operation preparation of the polymer film 3.
[0050] Select to deposit 1 micron copper foil on both sides at the same time, set the deposition rate to 10 microns / minute, and prepare the electrolytic deposition system. Start two sets of electrolytic copper foil deposition systems at the same time, and the two deposition rollers 2 rotate synchronously with the rotation speed of the rotating rollers on the unwinding mechanism 5 and the winding mechanism 4, and the rotation rate (i.e., the walking rate) is 10m / minute, so as to realize the preparation of composite copper foil with a thickness of 1 micron copper foil attached to the PE substrate.
[0051] The composite copper foil of the present application can significantly reduce the amount of metallic copper used, improve the strength and toughness of the copper foil, and at the same time does not reduce the conductivity of the copper foil. The currently developing composite copper foil technologies all require the use of expensive vacuum coating methods. The present application realizes the preparation of a new generation of composite copper foil that is low-cost, low-investment, and can be quickly connected with existing industries.
[0052] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A composite copper foil preparation system, characterized in that: The invention comprises at least two deposition rollers (2) arranged opposite to each other, each of the deposition rollers (2) being connected to a copper foil electrolytic deposition line (1), a reeling mechanism (5) and a reeling mechanism (4) being arranged on both sides of the deposition roller (2), and a polymer film (3) passing through a gap between the two deposition rollers (2) being wound around the reeling mechanism (5) and the reeling mechanism (4).
2. A composite copper foil preparation system according to claim 1, characterized in that: A tension adjustment mechanism for adjusting the tension of the polymer film (3) is provided between the unwinding mechanism (5) and the rewinding mechanism (4).
3. A composite copper foil preparation system according to claim 1, characterized in that: The two deposition rollers (2) are connected to an adjustment base capable of adjusting the gap between the two deposition rollers (2).
4. A composite copper foil preparation system according to claim 1, characterized in that: The unwinding mechanism (5) is provided with a glue coating device for coating the surface of the polymer film (3) with glue.
5. A method for preparing a composite copper foil, using the composite copper foil preparation system as claimed in claim 2, characterized in that: The preparation method comprises the following steps: S1, placing the rolled polymer film (3) on the unwinding mechanism (5), unfolding the polymer film (3) and pulling the polymer film (3) through the gap between the two deposition rollers (2), then winding the polymer film (3) on the winding mechanism (4), adjusting the tension adjustment mechanism to ensure that the polymer film (3) moves evenly and without deviation, and preparing and fixing the moving speed; S2, the copper foil electrolytic deposition line (1) is prepared, including preparation for electrolyte filtration and concentration adjustment, preparation for anode electrolytic copper plate, preparation for deposition roller (2) and preparation for electrolytic deposition power supply, and the power supply power is set according to the effective deposition area of the deposition roller (2) and the rotation speed of the deposition roller (2), so as to control the deposition rate; S3, checking the contact pressure between the deposition roller (2) and the polymer film (3), ensuring that there is sufficient pressing force between the copper foil on the deposition roller (2) and the polymer film (3), so that the bonding force between the copper foil and the polymer film (3) is greater than the bonding force of the copper foil on the deposition roller (2); S4, after the preparation and inspection are completed, the unwinding mechanism (5) and the rewinding mechanism (4) are started to unwind and rewind, and the copper foil electrolytic deposition line (1) works in sequence, the copper foil is deposited on the deposition roller (2) and transferred and pressed onto the polymer film (3), and the polymer film (3) peels the copper foil off the deposition roller (2) to form a composite copper foil; S5. When a composite copper foil roll is prepared, the copper foil electrolytic deposition line (1), the unwinding mechanism (5) and the rewinding mechanism (4) are stopped in sequence, thereby completing a process.
6. The method for preparing a composite copper foil according to claim 5, characterized in that: The walking speed is 0.01-100 m / min.
7. The method for preparing a composite copper foil according to claim 5, characterized in that: The deposition rate is 0.01-100 μm / min.
8. The method for preparing a composite copper foil according to claim 5, characterized in that: The bonding force between the copper foil and the polymer film (3) is twice or more the bonding force of the copper foil on the deposition roller (2).