Iridium composite coating titanium anode and preparation method thereof
The titanium plate is activated by electrochemical anodizing method and plating the tin antimony alloy layer, and then periodically plating is carried out to form an iridium composite plating layer, which solves the problems of weak binding force and insufficient stability of the iridium-coated titanium anode, and achieves high efficiency , low-cost electrode preparation improves electrochemical performance and service life.
Patent Information
- Application Number
- CN202410914139.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing iridium-coated titanium anode has weak coating bonding force, insufficient stability and complex preparation conditions.
The surface of the titanium plate is activated by electrochemical anodizing method, a titanium oxide layer is formed, and a tin antimony alloy layer is coated as an intermediate layer. Then periodically electroplating is performed on the tin antimony alloy layer to form an iridium composite plating layer, optimizing the iridium layer Microstructure and adhesion reduces iridium load and cost.
It improves the adhesion and stability of the coating, extends the service life of the electrode, reduces the load of precious metal elements, simplifies the preparation process, reduces the cost of the electrode, and improves the electrochemical performance.
Smart Images

Figure CN118932445A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochemistry, and in particular to an iridium composite-plated titanium anode and a preparation method thereof. Background Art
[0002] As a key component of various electrochemical technologies, titanium anodes are widely used in the fields of chlor-alkali industry, wastewater treatment, electrolytic organic synthesis, electroplating, energy conversion, etc. Among them, the iridium-coated titanium anode is the only anode that can meet the stability requirements of the local acidic environment of commercial electrolytic cells due to its excellent stability in acidic media. It is also the most widely used active anode in the field of wastewater treatment. The iridium-coated titanium anode has the characteristics of strong corrosion resistance, stable structure, and long working life. It is an excellent electrode material. At present, the iridium-coated titanium anodes sold on the market are mainly made by thermal decomposition, that is, by repeatedly brushing the iridium salt coating liquid and treating it at high temperature to decompose it into metal oxides. The electrodes prepared by thermal decomposition method have excellent stability, but the preparation process is cumbersome and requires high temperature. In addition, the electrode activity is not high and the iridium loading is large. Usually the precious metal content is ≥15g / m 2 In order to meet the requirements, the cost of electrodes is high and industrial applications are limited.
[0003] In addition to thermal decomposition, existing anode preparation technologies also include magnetron sputtering, physical / chemical vapor deposition, electrodeposition, sol-gel method, etc. Magnetron sputtering and physical / chemical vapor deposition techniques can produce nano-scale coatings and iridium oxides with good film-forming effects, but they have strict requirements on the process and rely on precision instruments and equipment, and are not suitable for large-scale electrode manufacturing. The raw materials of the sol-gel method are mostly metal organics, which are expensive and pose environmental and health risks. In contrast, the electrodeposition technology has mild preparation conditions, a high degree of mechanization, and controllable iridium loading.
[0004] Chinese patent CN108018583 discloses an electrolytic anode plate and its preparation method and application. The preparation method uniformly coats an intermediate layer coating liquid containing iridium and tin on a substrate, then uniformly electroplates an iridium-containing electroplating liquid onto the intermediate layer of the substrate, and obtains an electrolytic anode plate after drying. The prepared electrolytic anode plate has improved electrocatalytic activity, which is beneficial to the catalytic decomposition of water and is applied to electrolytic sludge dehydration, electrolytic water and power-to-gas conversion. The invention realizes the plating of an iridium oxide layer through electrodeposition technology. The prepared titanium anode has high electrochemical activity and can be applied to the preparation of titanium anodes of various specifications and shapes. It is a method for preparing iridium-based coated titanium anodes worthy of promotion. However, since the preparation of the intermediate layer of this method still adopts the form of coating-thermal decomposition of iridium coating liquid and tin coating liquid, high temperature is repeatedly required, which increases the consumption of iridium, and the stability of the prepared electrode is not analyzed. The technical solution has the disadvantages of weak coating bonding and insufficient stability. Therefore, it is necessary to improve the existing electrodeposition preparation technology of iridium oxide coated titanium anode, and provide a preparation method with simple operation, mild reaction conditions, stable electrochemical performance of the prepared electrode and low iridium loading. Summary of the invention
[0005] In view of this, the present invention proposes an iridium composite coated titanium anode and a preparation method thereof to solve the problems of weak coating bonding, insufficient stability and complex preparation conditions of the iridium-based coated titanium anode in the prior art.
[0006] The technical solution of the present invention is achieved in this way:
[0007] In a first aspect, the present invention provides a method for preparing an iridium composite-coated titanium anode, comprising the following steps:
[0008] S1, performing an anodic oxidation activation treatment on the titanium plate through an electrolytic reaction to obtain an activated titanium plate;
[0009] S2, coating the surface of the activated titanium plate with a tin-antimony coating by an electrodeposition method;
[0010] S3, using the titanium plate coated with the tin-antimony coating obtained in step S2 as an anode, periodic electroplating is performed to obtain an iridium composite coating titanium anode.
[0011] Directly performing the electroplating operation on the titanium plate may result in poor adhesion of the coating and easy to fall off. Therefore, in step S1 of the present invention, the surface of the titanium plate is first activated by an electrochemical anodizing method to increase the surface roughness of the titanium plate and improve the adhesion of the coating. The titanium oxide layer formed by anodizing not only provides more surface area to enhance the mechanical interlocking of the coating, but also enhances the corrosion resistance of the overall structure through its chemical stability, providing an ideal substrate for the tin-antimony coating. In step S2, a tin-antimony alloy layer is formed by an electroplating method, which, as an intermediate layer, can effectively serve as a bearing layer for the iridium layer, which helps the uniform deposition and adhesion of the iridium layer, reduces the use amount of the iridium layer, and reduces costs. The presence of the tin-antimony alloy layer can provide a more uniform and suitable surface for iridium deposition, optimizes the microstructure and adhesion of the iridium layer, and avoids direct deposition of iridium on the titanium oxide layer, which may cause uneven distribution of the iridium layer, affecting the performance and life of the anode. In step S3, iridium is further plated on the tin-antimony alloy coating to form a high-performance iridium composite coating titanium anode, which is conducive to a more uniform, dense and iridium layer with a specific crystal orientation through periodic electroplating. The anode preparation method provided by the present invention can effectively reduce the load of precious metal elements and extend the service life of the electrode, and has the characteristics of strong operability, mild preparation conditions, flexible structure and good electrochemical performance.
[0012] On the basis of the above technical solution, preferably, step S1 specifically includes:
[0013] S11, immersing the titanium plate in an etching solution for polishing;
[0014] S12. Use the polished titanium plate as the working electrode and graphite as the counter electrode to perform anodization in an activation solution.
[0015] More preferably, step S11 specifically includes: using a titanium plate as a base material, removing oil stains on the surface of the titanium plate by alkaline washing; then using sandpaper (mesh number greater than 1500 mesh) to polish the surface of the titanium plate, after cleaning and drying, immersing the titanium plate in an etching solution for polishing, and the processing time is 4 to 8 minutes.
[0016] More preferably, step S12 specifically includes: using the polished titanium plate as the working electrode and the graphite as the counter electrode, performing anodizing treatment by electrolysis reaction in an activation solution, wherein the electrolysis is constant voltage electrolysis, the electrolysis voltage is 20-30V, the electrolysis temperature is 40-45°C, and the electrolysis time is 2-3h.
[0017] Specifically, alkaline washing can completely remove grease and some organic matter on the surface of the titanium plate; sandpaper polishing can physically increase the surface roughness of the titanium plate, which is beneficial to improve the mechanical interlocking of the coating and enhance the bonding strength between the coating and the substrate; polishing with an acidic solution can remove the oxide layer and tiny impurities on the surface of the titanium plate, making the surface more uniform and smooth, while increasing the surface activity of the titanium plate at the microscopic level.
[0018] On the basis of the above technical solution, preferably, the etching solution is a mixture of two or more acidic solutions, and the activation solution includes a mixture of ammonium fluoride, hydrofluoric acid and an activation aid.
[0019] More preferably, the etching solution includes a mixture of any two or more of hydrofluoric acid, nitric acid, sulfuric acid, phosphoric acid, oxalic acid and hydrochloric acid; more preferably, the etching solution can be any one or more of 0.5-1.5wt.% hydrofluoric acid and 2.5-3.5wt.% nitric acid, 1.5-2.5wt.% sulfuric acid and 0.5-1.5wt.% hydrofluoric acid, 4.5-5.5wt.% phosphoric acid and 0.5-1.5wt.% hydrofluoric acid, 2.5-3.5wt.% oxalic acid and 0.5-1.5wt.% hydrofluoric acid. The present invention is not limited to this, as long as it can achieve polishing of the surface of the titanium plate.
[0020] More preferably, the activation aid includes a buffer and a surfactant, wherein the buffer can be any one or more of acetic acid, citric acid, and boric acid, and the surfactant can be any one or more of polyethylene glycol and povidone. More preferably, the activation aid includes glacial acetic acid and polyethylene glycol, and the composition of the activation solution includes: 5-8 mg / L of ammonium fluoride, 0.3-0.5 wt.% of hydrofluoric acid, 0.1-0.3 wt.% of glacial acetic acid, and 0.04-0.06 wt.% of polyethylene glycol.
[0021] During the anodizing process, the titanium plate acts as the anode, and the titanium element loses electrons under the action of the electric field and combines with the oxygen ions in the electrolyte to form titanium oxide. Fluoride ions provided by ammonium fluoride and hydrofluoric acid help to form a dense and uniform oxide film on the anode surface; buffers can provide good pH buffering capacity, maintain the stability of the electrolyte environment, and help control the oxidation process; surfactants can improve the uniform distribution of current, ensure the uniform formation of the oxide film, and avoid local over-oxidation.
[0022] On the basis of the above technical scheme, preferably, in step S2, the electrodeposition method specifically includes using the activated titanium plate as the working electrode, the platinum sheet as the counter electrode, and the silver-silver chloride electrode as the reference electrode, and performing electrodeposition in a tin-antimony electroplating solution to obtain a titanium plate coated with a tin-antimony coating.
[0023] More preferably, the electrodeposition is constant current electrodeposition, and the deposition current density is -5 to -10 mA / cm 2 The deposition temperature is 5-40°C and the deposition time is 15-30min.
[0024] Specifically, during the electrodeposition process, tin and antimony ions are reduced on the surface of the titanium plate under the drive of electric current to form a tin-antimony coating. The tin-antimony coating provides the necessary mechanical and chemical properties to support the electrocatalytic activity of the subsequent iridium layer; at the same time, it helps to deposit the iridium layer uniformly and improve the adhesion of the iridium layer, thereby reducing the amount of iridium used and reducing costs. By using a constant current density (-5 to -10 mA / cm 2 ), the growth rate and thickness of the coating can be controlled, ensuring the uniformity of the alloy layer and avoiding the increase of roughness or sintering that may be caused by excessive current density. Lower temperatures help slow the deposition rate, thereby improving the uniformity and compactness of the coating. Controlling the deposition time can accurately control the total thickness of the coating, ensuring sufficient coverage while avoiding unnecessary material waste.
[0025] On the basis of the above technical solution, preferably, the tin-antimony electroplating solution comprises at least a soluble tin salt and a soluble antimony salt, the concentration of the soluble tin salt is 20-40 g / L, and the concentration of the soluble antimony salt is 5-10 g / L.
[0026] More preferably, the soluble tin salt includes any one or more of stannous sulfate, tin fluoroborate, tin chloride and tin nitrate; the soluble antimony salt includes any one or more of potassium antimony tartrate, antimony chloride and antimony nitrate.
[0027] The tin-antimony electroplating solution also includes a mixture of fluoroboric acid, hydrofluoric acid, p-diphenol and gelatin. More preferably, the tin-antimony electroplating solution includes stannous sulfate, potassium antimony tartrate, fluoroboric acid, hydrofluoric acid, p-diphenol and gelatin, wherein the concentration of stannous sulfate is 20-40 g / L; the concentration of potassium antimony tartrate is 5-10 g / L; the concentration of fluoroboric acid is 80-100 g / L; the concentration of hydrofluoric acid is 2-5 g / L; the concentration of p-diphenol is 1-2 g / L; and the concentration of gelatin is 0.5-1 g / L.
[0028] Specifically, soluble tin salt and soluble antimony salt provide tin ions and antimony ions, respectively, to form a tin-antimony coating, and additives such as gelatin and p-diphenol help to control the crystal structure and surface morphology of the coating, thereby improving its mechanical and chemical properties.
[0029] On the basis of the above technical solution, preferably, step S2 further includes thermal oxidation treatment of the tin-antimony coating, specifically including:
[0030] After the electrodeposition treatment, the titanium plate coated with the tin-antimony coating is heated to 450-550° C. at a rate of 8-12° C. / min, heated at a constant temperature for 1.5-2.5 hours, and cooled to 25-27° C. to obtain a titanium plate with a tin-antimony oxide coating.
[0031] Specifically, during the heat treatment process, the coating material undergoes lattice rearrangement and phase transformation at high temperature, which helps to reduce internal defects such as dislocations and microcracks. Constant temperature heating and subsequent slow cooling further ensure the uniformity and stability of the coating. Annealing treatment can eliminate the stress generated during the electrodeposition process, optimize the crystal structure of the tin-antimony alloy, and improve its corrosion resistance and mechanical properties; the treated coating has better crystallinity, which helps to improve its overall performance, especially the long-term stability and durability when used as an electrochemical anode.
[0032] On the basis of the above technical solution, preferably, the periodic electroplating in step S3 specifically includes:
[0033] A titanium plate with a tin-antimony oxide coating was used as a working electrode, a platinum sheet was used as a counter electrode, and a mercury-mercury oxide electrode was used as a reference electrode. Cyclic voltammetry electrodeposition was carried out in an iridium plating solution with a scanning voltage of -0.6V to 0.6V, a scanning rate of 1 to 5mV / s, and a deposition temperature of 30 to 35°C.
[0034] Iridium is deposited on the tin-antimony alloy coating using cyclic voltammetry to form an iridium composite coating, which enhances the electrocatalytic activity and durability of the anode. Within the set potential range, iridium ions are reduced on the cathode (working electrode) to form an iridium metal coating. Cyclic scanning of the potential helps eliminate surface unevenness and promotes uniformity of coating growth; cyclic voltammetry allows repeated scanning of the potential during the electroplating process, which helps to form a more uniform and dense iridium coating.
[0035] On the basis of the above technical solution, preferably, the iridium electroplating solution comprises a mixture of two or more iridium salts, potassium oxalate and a second additive, and the pH value of the iridium electroplating solution is 10 to 10.5.
[0036] More preferably, the iridium salt includes but is not limited to iridium trichloride, chloroiridic acid, potassium chloroiridate, sodium chloroiridate and iridium sulfate; the second additive includes one or more of potassium carbonate, sodium carbonate, sodium hydroxide, potassium hydroxide and sodium acetate. More preferably, the iridium electroplating solution includes 1.3-2.5 g / L of iridium salt; 3-6 g / L of potassium oxalate; and 0.2-0.5 g / L of the second additive.
[0037] Iridium salt is used to provide the necessary iridium ions for electrodeposition; potassium oxalate, as a complexing agent, helps stabilize the iridium ions in the electroplating solution and reduce the roughness and unevenness of the coating caused by direct deposition of iridium ions; the alkaline environment is controlled by the second additive, which helps to stabilize and effectively reduce the iridium ions while reducing possible excessive hydrogen precipitation, which helps to prevent the formation of bubbles and holes in the coating.
[0038] On the basis of the above technical solution, preferably, step S3 further includes high-temperature sintering. After the periodic electroplating is completed, the electroplated titanium plate is calcined at 250-350° C. for 1.5-2.5 hours to obtain an iridium composite-coated titanium anode.
[0039] During the sintering process, a certain diffusion and bonding will occur at the interface between the iridium layer and the tin-antimony alloy layer, thereby enhancing the adhesion and corrosion resistance of the overall coating; high-temperature treatment can also improve the crystal structure of the iridium layer, further improving the mechanical strength and electrochemical properties of the anode.
[0040] In a second aspect, the present invention provides an iridium composite-coated titanium anode, which is prepared by the preparation method described above.
[0041] The iridium composite-coated titanium anode and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:
[0042] (1) The titanium substrate surface is activated by anodizing, which provides more active sites for the subsequent coating, greatly enhances the bonding force between the additional coating and the substrate material, and further introduces a tin antimony oxide coating by direct electrodeposition technology to provide support for the adhesion of the subsequent iridium oxide coating, thereby avoiding the problem of coating shedding, rapid dissolution, and insufficient electrode stability caused by the weak bonding force between iridium oxide and the titanium substrate. At the same time, the titanium substrate is protected from being corroded by acidic media during the electrolysis process, thereby generating a non-conductive TiO2 layer that causes electrode passivation failure, further extending the service life of the electrode;
[0043] (2) The iridium oxide layer is plated by periodic electroplating at a low scanning speed, which has a higher deposition efficiency, a dense coating, and no dendrite formation, thereby having a large electrochemically active surface area and better electrode electrocatalytic activity, which is beneficial to the improvement of electrolysis efficiency in practical applications;
[0044] (3) The electrode preparation process of the present invention is short and the conditions are mild. The electrode anodic oxidation activation treatment and the tin-antimony layer electroplating are both carried out in the same electrolytic cell, without the need to disassemble and reorganize the anode and add additional consumables. In addition, the iridium load of the prepared electrode is small, and the electrode cost is greatly reduced. At the same time, the equipment requirements are low, the operation is simple, and it has mechanization potential, which can further expand the industrial application of iridium-coated titanium anodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0046] Figure 1 The present invention is a flow chart for preparing the iridium composite-coated titanium anode;
[0047] Figure 2 The microscopic morphology of the titanium electrodes prepared in Example 6, Example 7, Comparative Example 1 and Comparative Example 2 of the present invention.
[0048] Figure 3 XRD comparison diagram of the titanium electrodes prepared in Example 6, Example 7, Comparative Example 1 and Comparative Example 2 of the present invention
[0049] Figure 4 This is the XPS characterization diagram of the iridium composite-coated titanium anode prepared in Example 5 of the present invention.
[0050] Figure 5 It is a comparison diagram of LSV curves of titanium electrodes prepared in Example 6, Example 7, Comparative Example 1 and Comparative Example 2 of the present invention.
[0051] Figure 6 It is a comparison chart of the enhanced life test curves of the titanium electrodes prepared in Example 6, Example 7, Comparative Example 1 and Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0052] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Example 1
[0054] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof, such as Figure 1 As shown, the specific steps include:
[0055] (1) An industrial-grade titanium plate (TA2) was used as the substrate material. After being soaked in a 5 wt.% sodium hydroxide solution for 10 min, the surface oil stains were removed by rinsing with clean water.
[0056] (2) An anodic oxidation activation solution was prepared, wherein the ammonium fluoride content was 6 mg / L, the hydrofluoric acid content was 0.4 wt.%, and 0.2 wt.% glacial acetic acid and 0.05 wt.% polyethylene glycol were added.
[0057] (3) An anodic oxidation activation treatment is carried out in an electrolytic cell using a two-electrode system, with the polished titanium substrate in step (1) being the working electrode, the platinum sheet being the counter electrode, and the activation solution prepared in step (2) being the electrolyte. Constant voltage electrolysis is adopted, the electrolysis voltage is 20 V, the electrolysis temperature is 45° C., and the electrolysis time is 2 h. After the anodic oxidation activation treatment is completed, the activation solution in the electrolytic cell is discharged, and the electrolytic cell, the pipeline and the electrode surface are rinsed with clean water, wherein the activation solution is centrally sealed and stored for next use.
[0058] (4) Prepare an iridium electroplating solution with an iridium salt concentration of 1.5 g / L, which is a mixture of iridium trichloride and chloroiridic acid in a molar ratio of 3:1, and a potassium oxalate concentration of 6 g / L. Then add 1 to 2 mL of hydrogen peroxide and stir thoroughly to mix evenly. Finally, add an appropriate amount of potassium hydroxide to adjust the pH of the solution to 10 to 10.5, and place it in a 40°C water bath for 4 days to stabilize it. Use the titanium substrate activated by anodization in step (3) as the working electrode, the platinum sheet as the counter electrode, and the mercury-mercury oxide electrode as the reference electrode to perform electrodeposition in the iridium electroplating solution.
[0059] Cyclic voltammetry was used for periodic electroplating, with a scanning potential range of -0.6 to 0.6 V, a scanning rate of 5 mV / s, a cycle period of 20 turns, and a deposition temperature of room temperature.
[0060] The iridium concentration in the plating solution before and after electroplating was measured by inductively coupled plasma optical emission spectrometry (ICP-OES), and the iridium loading of the electrode was calculated as the difference between the two values. The final iridium loading was 0.25 mg / cm 2 .
[0061] (5) After the electrodeposition is completed, the electrode is taken out and the surface is rinsed with clean water, and then it is dried by blowing hot air or baking under an infrared lamp for 10 to 15 minutes, and then placed in a muffle furnace at a constant temperature of 300°C for 2 hours. The equipment is turned off, and the electrode is taken out after cooling to room temperature, thereby completing the preparation of the composite-coated titanium anode.
[0062] Example 2
[0063] The present embodiment provides an iridium composite-coated titanium anode and a preparation method thereof. The specific preparation method is the same as that of Example 1, except that: after removing the oil stains on the surface of the titanium plate in step (1), the titanium plate is polished with sandpaper (mesh size > 1500 mesh) until the surface is smooth, washed with clean water, and then immersed in a mixed aqueous solution of 1wt.% hydrofluoric acid and 3wt.% nitric acid and allowed to stand for 8 minutes for polishing. And after step (3), step (4) is added to prepare a tin-antimony coating, that is, a tin-antimony electroplating solution with a stannous sulfate concentration of 30g / L and a potassium antimony tartrate concentration of 5g / L is prepared, and fluoroboric acid, hydrofluoric acid, p-diphenol and gelatin are added in sequence, corresponding to the concentration ranges of 90g / L, 3g / L, 1.5g / L and 0.8g / L, respectively, and stirred thoroughly to make them evenly mixed. Add the tin-antimony electroplating solution to the cleaning electrolytic cell in step (3), and directly perform electrodeposition using a constant current, with a deposition current density of -5mA / cm 2 , the deposition temperature is 25℃, and the deposition time is 30min. After the electroplating is completed, the plating solution in the tank is discharged and the electrolytic tank equipment and pipelines are cleaned. The tin-antimony plating solution is centrally sealed and stored for standby use.
[0064] Example 3
[0065] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof. The specific preparation method is the same as that of Embodiment 2, except that: after step (4) is completed, the tin-antimony coating is further subjected to thermal oxidation treatment, that is, the tin-antimony coating titanium anode is placed in a muffle furnace for thermal oxidation treatment, an air atmosphere is selected, the heating rate is 10°C / min, and after reaching 500°C, the heating is continued and maintained at the temperature for 2 hours, and then the equipment is turned off, and the electrode is taken out after cooling to room temperature. At this time, the tin-antimony coating is completely converted into a tin-antimony oxide coating. Then, the tin-antimony oxide-coated titanium anode is used as the working electrode for subsequent iridium electrodeposition.
[0066] Example 4
[0067] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof, which specifically includes the following steps:
[0068] (1) An industrial-grade titanium plate (TA2) was used as the substrate material. After being soaked in a 5 wt.% sodium hydroxide solution for 10 min, the titanium plate was rinsed with clean water to remove surface oil stains. The titanium plate was polished with sandpaper (mesh size > 1500 mesh) until the surface was smooth, rinsed with clean water, and then immersed in a mixed aqueous solution of 1 wt.% hydrofluoric acid and 3 wt.% nitric acid for 6 min for polishing.
[0069] (2) An anodic oxidation activation solution was prepared, wherein the ammonium fluoride content was 8 mg / L, the hydrofluoric acid content was 0.3 wt.%, and 0.2 wt.% glacial acetic acid and 0.05 wt.% polyethylene glycol were added.
[0070] (3) An anodic oxidation activation treatment is performed in an electrolytic cell using a two-electrode system, with the polished titanium substrate in step (1) being the working electrode, the platinum sheet being the counter electrode, and the activation solution prepared in step (2) being the electrolyte. Constant voltage electrolysis is performed, with an electrolysis voltage of 30 V, an electrolysis temperature of 45° C., and an electrolysis time of 2 h. After the anodic oxidation activation treatment is completed, the activation solution in the electrolytic cell is discharged, and the electrolytic cell, the pipeline, and the electrode surface are rinsed with clean water, wherein the activation solution is centrally sealed and stored for next use.
[0071] (4) Prepare a tin-antimony electroplating solution with a stannous sulfate concentration of 30 g / L and an antimony potassium tartrate concentration of 5 g / L, and add fluoroboric acid, hydrofluoric acid, p-diphenol and gelatin in sequence, corresponding to the concentration range of 90 g / L, 3 g / L, 1.5 g / L and 0.8 g / L, respectively, and stir well to make them uniformly mixed. Add the tin-antimony electroplating solution to the cleaned electrolytic cell in step (3), and directly perform electrodeposition using a constant current, with a deposition current density of -5 mA / cm 2 , the deposition temperature is 25℃, and the deposition time is 30min. After the electroplating is completed, the plating solution in the tank is discharged and the electrolytic tank equipment and pipelines are cleaned. The tin-antimony plating solution is centrally sealed and stored for standby use.
[0072] The tin-antimony coated titanium anode is subjected to thermal oxidation treatment, that is, the tin-antimony coated titanium anode is placed in a muffle furnace for thermal oxidation treatment, an air atmosphere is selected, the heating rate is 10°C / min, and after reaching 500°C, heating is continued and maintained at this temperature for 2 hours, and then the equipment is turned off, and the electrode is taken out after cooling to room temperature. At this time, the tin-antimony coating is completely converted into a tin-antimony oxide coating.
[0073] (5) Prepare an iridium electroplating solution with an iridium salt concentration of 2.5 g / L, which is a mixture of iridium trichloride and chloroiridic acid in a molar ratio of 3:1, and a potassium oxalate concentration of 10 g / L. Then add 1 to 2 mL of hydrogen peroxide and stir thoroughly to mix evenly. Finally, add an appropriate amount of potassium hydroxide to adjust the solution pH to 10 to 10.5, and place it in a 40°C water bath for 4 days to stabilize it. Electrodeposition is performed in the iridium electroplating solution using the tin antimony oxide-coated titanium anode prepared in step (4) as the working electrode, the platinum sheet as the counter electrode, and the mercury-mercury oxide electrode as the reference electrode.
[0074] Cyclic voltammetry was used for periodic electroplating, with a scanning potential range of -0.6 to 0.6 V, a scanning rate of 5 mV / s, a cycle period of 30 circles, and a deposition temperature of room temperature.
[0075] The iridium concentration in the plating solution before and after electroplating was measured by inductively coupled plasma optical emission spectrometry (ICP-OES), and the iridium loading of the electrode was calculated as the difference between the two values. The final iridium loading was 0.42 mg / cm 2 .
[0076] (6) After the electrodeposition is completed, the electrode is taken out and the surface is rinsed with clean water, and then it is dried by blowing hot air or baking under an infrared lamp for 10 to 15 minutes, and then placed in a muffle furnace at a constant temperature of 300°C for 2 hours. The equipment is turned off, and the electrode is taken out after cooling to room temperature, thereby completing the preparation of the composite-coated titanium anode.
[0077] Example 5
[0078] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof. The specific preparation method is the same as that of Embodiment 4, except that: in step (5), cyclic voltammetry is used for periodic electroplating, the scanning potential range is -0.6 to 0.6 V, the scanning rate is 5 mV / s, the cycle period is 40 cycles, the deposition temperature is room temperature, and the final iridium loading is 0.5 mg / cm 2 .
[0079] Example 6
[0080] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof, which specifically includes the following steps:
[0081] (1) An industrial-grade titanium plate (TA2) was used as the substrate material. After being soaked in a 5 wt.% sodium hydroxide solution for 10 min, the titanium plate was rinsed with clean water to remove surface oil stains. The titanium plate was polished with sandpaper (mesh size > 1500 mesh) until the surface was smooth, rinsed with clean water, and then immersed in a mixed aqueous solution of 1 wt.% hydrofluoric acid and 2 wt.% sulfuric acid for 4 to 8 min for polishing.
[0082] (2) An anodic oxidation activation solution was prepared, wherein the ammonium fluoride content was 5 mg / L, the hydrofluoric acid content was 0.3 wt.%, and 0.1 wt.% glacial acetic acid and 0.04 wt.% polyethylene glycol were added.
[0083] (3) An anodic oxidation activation treatment is carried out in an electrolytic cell using a two-electrode system, with the polished titanium substrate in step (1) being the working electrode, the platinum sheet being the counter electrode, and the activation solution prepared in step (2) being the electrolyte. Constant voltage electrolysis is adopted, the electrolysis voltage is 20 V, the electrolysis temperature is 40° C., and the electrolysis time is 2.5 h. After the anodic oxidation activation treatment is completed, the activation solution in the electrolytic cell is discharged, and the electrolytic cell, the pipeline and the electrode surface are rinsed with clean water, wherein the activation solution is centrally sealed and stored for next use.
[0084] (4) Prepare a tin-antimony electroplating solution with a stannous sulfate concentration of 20 g / L and an antimony potassium tartrate concentration of 8 g / L, and add fluoroboric acid, hydrofluoric acid, p-diphenol and gelatin in sequence, corresponding to the concentration range of 80 g / L, 2 g / L, 1 g / L and 0.5 g / L, respectively, and stir well to make them uniformly mixed. Add the tin-antimony electroplating solution to the cleaned electrolytic cell in step (3), and directly perform electrodeposition using a constant current, with a deposition current density of -8 mA / cm2 , the deposition temperature is 5°C, and the deposition time is 15 minutes. After the electroplating is completed, the plating solution in the tank is discharged and the electrolytic tank equipment and pipelines are cleaned. The tin-antimony plating solution is centrally sealed and stored for standby use.
[0085] The tin-antimony coated titanium anode is subjected to thermal oxidation treatment, that is, the tin-antimony coated titanium anode is placed in a muffle furnace for thermal oxidation treatment, an air atmosphere is selected, the heating rate is 8°C / min, and after reaching 450°C, heating is continued and maintained at this temperature for 1.5 hours, and then the equipment is turned off, and the electrode is taken out after cooling to room temperature. At this time, the tin-antimony coating is completely converted into a tin-antimony oxide coating.
[0086] (5) Prepare an iridium electroplating solution with an iridium salt concentration of 1.3 g / L, which is a mixture of iridium trichloride and chloroiridic acid in a molar ratio of 3:1, and a potassium oxalate concentration of 3 g / L, then add 1-2 mL of hydrogen peroxide, stir thoroughly to mix evenly, and finally add an appropriate amount of potassium hydroxide to adjust the solution pH to 10-10.5, and place it in a 40°C water bath for 4 days to stabilize it. Use the tin antimony oxide-coated titanium anode prepared in step (4) as the working electrode, the platinum sheet as the counter electrode, and the mercury-mercury oxide electrode as the reference electrode to perform electrodeposition in the iridium electroplating solution.
[0087] Cyclic voltammetry was used for periodic electroplating, with a scanning potential range of -0.6 to 0.6 V, a scanning rate of 1 mV / s, a cycle period of 40 turns, and a deposition temperature of room temperature.
[0088] The iridium concentration in the plating solution before and after electroplating was measured by inductively coupled plasma optical emission spectrometry (ICP-OES), and the iridium loading of the electrode was calculated as the difference between the two values. The final iridium loading was 0.5 mg / cm 2 .
[0089] (6) After the electrodeposition is completed, the electrode is taken out and the surface is rinsed with clean water, and then it is dried by blowing hot air or baking under an infrared lamp for 10 to 15 minutes, and then placed in a muffle furnace at a constant temperature of 250°C for 1.5 hours. The equipment is turned off, and the electrode is taken out after cooling to room temperature, thereby completing the preparation of the composite-coated titanium anode.
[0090] Example 7
[0091] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof, which specifically includes the following steps:
[0092] (1) An industrial-grade titanium plate (TA2) was used as the substrate material. After being soaked in a 5 wt.% sodium hydroxide solution for 10 min, the titanium plate was rinsed with clean water to remove surface oil stains. The titanium plate was polished with sandpaper (mesh size > 1500 mesh) until the surface was smooth, rinsed with clean water, and then immersed in a mixed aqueous solution of 1.5 wt.% hydrofluoric acid and 2.5 wt.% nitric acid for 4 to 8 min for polishing.
[0093] (2) An anodic oxidation activation solution was prepared, wherein the ammonium fluoride content was 8 mg / L, the hydrofluoric acid content was 0.5 wt.%, and 0.3 wt.% glacial acetic acid and 0.06 wt.% polyethylene glycol were added.
[0094] (3) An anodic oxidation activation treatment is performed in an electrolytic cell using a two-electrode system, with the polished titanium substrate in step (1) being the working electrode, the platinum sheet being the counter electrode, and the activation solution prepared in step (2) being the electrolyte. Constant voltage electrolysis is performed, with an electrolysis voltage of 25 V, an electrolysis temperature of 45° C., and an electrolysis time of 3 h. After the anodic oxidation activation treatment is completed, the activation solution in the electrolytic cell is discharged, and the electrolytic cell, the pipeline, and the electrode surface are rinsed with clean water, wherein the activation solution is centrally sealed and stored for next use.
[0095] (4) Prepare a tin-antimony electroplating solution with a tin fluoroborate concentration of 40 g / L and an antimony potassium tartrate concentration of 10 g / L, and add fluoroboric acid, hydrofluoric acid, p-diphenol and gelatin in sequence, corresponding to the concentration range of 100 g / L, 5 g / L, 2 g / L and 1 g / L, respectively, and stir well to make them uniformly mixed. Add the tin-antimony electroplating solution to the cleaned electrolytic cell in step (3), and directly perform electrodeposition using a constant current, with a deposition current density of -10 mA / cm 2 , the deposition temperature is 40℃, and the deposition time is 25min. After the electroplating is completed, the plating solution in the tank is discharged and the electrolytic tank equipment and pipelines are cleaned. The tin-antimony plating solution is centrally sealed and stored for standby use.
[0096] The tin-antimony coated titanium anode is subjected to thermal oxidation treatment, that is, the tin-antimony coated titanium anode is placed in a muffle furnace for thermal oxidation treatment, an air atmosphere is selected, the heating rate is 12°C / min, and after reaching 550°C, heating is continued and maintained at this temperature for 2.5 hours, and then the equipment is turned off, and the electrode is taken out after cooling to room temperature. At this time, the tin-antimony coating is completely converted into a tin-antimony oxide coating.
[0097] (5) Prepare an iridium electroplating solution with an iridium salt concentration of 2.0 g / L, which is a mixture of iridium trichloride and potassium chloroiridate in a molar ratio of 3:1, and a potassium oxalate concentration of 6 g / L. Then add 1 to 2 mL of hydrogen peroxide, stir thoroughly to mix evenly, and finally add an appropriate amount of potassium hydroxide to adjust the solution pH to 10 to 10.5, and place it in a 40°C water bath for 4 days to stabilize it. Electrodeposition is carried out in the iridium electroplating solution using the tin antimony oxide-coated titanium anode prepared in step (4) as the working electrode, the platinum sheet as the counter electrode, and the mercury-mercury oxide electrode as the reference electrode.
[0098] Cyclic voltammetry was used for periodic electroplating, with a scanning potential range of -0.6 to 0.6 V, a scanning rate of 2.5 mV / s, a cycle period of 40 turns, and a deposition temperature of room temperature.
[0099] The iridium concentration in the plating solution before and after electroplating was measured by inductively coupled plasma optical emission spectrometry (ICP-OES), and the iridium loading of the electrode was calculated as the difference between the two values. The final iridium loading was 0.5 mg / cm 2 .
[0100] (6) After the electrodeposition is completed, the electrode is taken out and the surface is rinsed with clean water, and then it is dried by blowing hot air or baking under an infrared lamp for 10 to 15 minutes, and then placed in a muffle furnace at a constant temperature of 350°C for 2.5 hours. The equipment is turned off, and the electrode is taken out after cooling to room temperature, thereby completing the preparation of the composite-coated titanium anode.
[0101] Example 8
[0102] The present embodiment provides an iridium composite-coated titanium anode and a preparation method thereof. The specific preparation method is the same as that of Example 5, except that: in step (5), the periodic electroplating is replaced by constant voltage electrodeposition. The constant voltage has an electrolysis voltage of 0.6 V, a scanning rate of 5 mV / s, and a deposition temperature of room temperature.
[0103] Example 9
[0104] The present embodiment provides an iridium composite-coated titanium anode and a preparation method thereof. The specific preparation method is the same as that of Example 5, except that: in step (5), cyclic voltammetry is used for periodic electroplating, the scanning potential range is -0.9 to 0.9 V, the scanning rate is 7 mV / s, the cycle period is 40 turns, and the deposition temperature is room temperature.
[0105] Example 10
[0106] This embodiment provides an iridium composite-coated titanium anode and a preparation method thereof. The specific preparation method is the same as that of Embodiment 5, except that: in step (5), potassium hydroxide is not added to the iridium electroplating solution, and its pH value is 6-8.
[0107] Comparative Example 1
[0108] The present comparative example provides an iridium titanium oxide anode and a preparation method thereof, which specifically comprises the following steps: the iridium titanium oxide anode is prepared by direct electrodeposition, specifically adopting a three-electrode system, wherein a titanium electrode etched by 10% boiling oxalic acid is a working electrode, a platinum sheet electrode is a counter electrode, a mercury-mercury oxide electrode is a reference electrode, the electrolyte is the iridium electroplating solution prepared in step (5) of Example 3, the electrodeposition voltage is 0.6-0.7V, and the current density is 0.1-0.5mA / cm 2 , deposited for a certain period of time until the iridium loading is 0.5 mg / cm 2 When the temperature reaches 300 °C, the electrode is taken out, rinsed with clean water and dried, and then heated in a muffle furnace at a constant temperature of 300 °C for 2 h. The equipment is turned off and the electrode is taken out after cooling to room temperature to complete the preparation of the iridium titanium oxide anode.
[0109] Comparative Example 2
[0110] This comparative example provides an iridium-tantalum coated titanium anode, which is prepared by a traditional brush coating method, using a classic iridium-tantalum coating liquid formula, and completing the electrode preparation by repeatedly brushing the coating liquid-thermal decomposition 5 to 6 times, wherein the coating iridium loading is 0.5 mg / cm 2 about.
[0111] Performance Testing
[0112] The enhanced life test is used to characterize the electrode stability. The potential change with time at a given current density is monitored by an electrochemical workstation or a DC power supply. The experiment is terminated with the potential as an indicator. The electrode operation time is the enhanced life (ALT). The test is carried out in an electrolytic cell under the following test conditions: the current density is 250mA / cm 2 , the temperature was room temperature, and the electrolyte was 0.5 mol / L H2SO4 solution. The test results are shown in Table 1.
[0113] Table 1
[0114]
[0115]
[0116] It can be seen from Table 1 that, when comparing Examples 1 to 3, the iridium composite-coated titanium anode prepared in Example 3 has a higher strengthening life under the same iridium loading, indicating that polishing treatment, the addition of tin-antimony coating and its thermal oxidation treatment will affect the strengthening life of the titanium anode, especially the addition of tin-antimony coating. Comparison of Examples 3 to 5 shows that the number of periodic cyclic electroplating cycles will affect the iridium loading, and then affect the strengthening life of the iridium composite-coated titanium anode, and the two are positively correlated. Comparison of Examples 5 to 7 shows that the iridium composite-coated titanium electrodes prepared by the technical solution of the present invention all have a higher strengthening life. Comparison of Example 5 and Example 8 shows that periodic cyclic electroplating treatment can improve the strengthening life of the iridium composite-coated titanium electrode. Comparison of Example 5 and Examples 9 and 10 shows that the process parameters of periodic cyclic electroplating treatment will affect the strengthening life of the iridium composite-coated titanium electrode.
[0117] The surface morphology of the prepared iridium composite-coated titanium electrode was observed by scanning electron microscopy (SEM). Figure 2 As shown, the figure shows the electrode surface of Example 6 and Example 7 magnified 7000 times. It can be seen from the figure that compared with the direct electrodeposition of iridium oxide electrodes, the grain size of the electrodeposited iridium oxide designed by the composite coating is significantly reduced to the nanometer level, and the surface of the deposited layer is smooth and uniform, and is more closely integrated with the base to form an integrated structure.
[0118] The microscopic crystal structure of the prepared iridium composite coating titanium electrode was observed by X-ray diffractometer (XRD) and compared with Comparative Examples 1 and 2. Figure 3 As shown, the iridium composite-coated titanium anode (Examples 6 and 7) shows a peak of crystalline SnO2 in addition to the peak of rutile phase IrO2. The direct electrodeposition of iridium oxide electrode (Comparative Example 2) shows a peak of TiO2, which may be due to the loose bonding between the coating and the substrate and the oxidation of the substrate during the heat treatment process, which means its poor stability.
[0119] X-ray photoelectron spectroscopy (XPS) was used to analyze the chemical state of the elements on the electrode surface and determine the microstructure of the catalytic layer. Figure 4 The XPS graph of the iridium composite-coated titanium anode prepared in Example 5 is shown. It can be seen from the figure that the surface of the composite coating is composed of iridium oxide, tin oxide and trace antimony oxide, proving that the composite coating was successfully prepared.
[0120] The titanium anodes prepared in Examples 6 and 7 and Comparative Examples 1 and 2 were tested for their electrocatalytic water decomposition performance using a three-electrode system, with the electrolyte being a 0.5 mol / L sulfuric acid solution. Figure 5 The electrocatalytic performance test graphs of the iridium composite-coated titanium anodes of Examples 6 and 7 and Comparative Examples 1 and 2 are shown. It can be seen from the graph that compared with the electrodes prepared by the traditional brush coating method and the electrodes prepared by the direct electrodeposition method (with the same iridium loading), the iridium composite-coated electrodes show a higher apparent current density, proving that their electrocatalytic activity is better than that of the brush coating electrodes and the direct electrodeposition electrodes, and their electrocatalytic efficiency is high.
[0121] Figure 6 The enhanced life test diagram of the iridium composite-coated titanium anode of Examples 6 and 7 and Comparative Examples 1 and 2 is shown. It can be seen from the figure that the iridium composite-coated electrodes prepared in Examples 6 and 7 can operate stably for about 600 hours, which is comparable to the stability level of electrodes prepared by the traditional thermal decomposition method. However, when the direct electrodeposition electrode operates for less than 20 hours, the potential begins to rise sharply and the electrode fails.
[0122] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an iridium composite-coated titanium anode, characterized in that: The following steps are involved: S1, performing an anodic oxidation activation treatment on the titanium plate through an electrolytic reaction to obtain an activated titanium plate; S2, coating the surface of the activated titanium plate with a tin-antimony coating by an electrodeposition method; S3, using the titanium plate coated with the tin-antimony coating obtained in step S2 as an anode, periodic electroplating is performed to obtain an iridium composite coating titanium anode.
2. The method for preparing an iridium composite-coated titanium anode according to claim 1, characterized in that: Step S1 specifically includes: S11, immersing the titanium plate in an etching solution for polishing; S12. Use the polished titanium plate as the working electrode and graphite as the counter electrode to perform anodization in an activation solution.
3. The method for preparing an iridium composite-coated titanium anode according to claim 2, characterized in that: The etching solution includes at least two acidic solutions, and the activation solution includes a mixture of ammonium fluoride, hydrofluoric acid and an activation aid.
4. The method for preparing an iridium composite-coated titanium anode according to claim 2, characterized in that: In step S2, the electrodeposition method specifically includes: using the activated titanium plate as the working electrode, the platinum sheet as the counter electrode, and the silver-silver chloride electrode as the reference electrode, and performing electrodeposition in a tin-antimony electroplating solution to obtain a titanium plate coated with a tin-antimony coating, wherein the electrodeposition is a constant current electrodeposition, and the deposition current density is -5 to -10 mA / cm 2 The deposition temperature is 5-40°C and the deposition time is 15-30min.
5. The method for preparing an iridium composite-coated titanium anode according to claim 4, characterized in that: The tin-antimony electroplating solution at least includes a soluble tin salt and a soluble antimony salt. The concentration of the soluble tin salt is 20-40 g / L, and the concentration of the soluble antimony salt is 5-10 g / L.
6. The method for preparing an iridium composite-coated titanium anode according to claim 4, characterized in that: Step S2 also includes thermal oxidation treatment of the tin-antimony coating, specifically including: After the electrodeposition treatment, the titanium plate coated with the tin-antimony coating is heated to 450-550° C. at a rate of 8-12° C. / min, heated at a constant temperature for 1.5-2.5 hours, and cooled to 25-27° C. to obtain a titanium plate with a tin-antimony oxide coating.
7. The method for preparing an iridium composite-coated titanium anode according to claim 1, characterized in that: The periodic electroplating in step S3 specifically includes: A titanium plate with a tin-antimony oxide coating was used as a working electrode, a platinum sheet was used as a counter electrode, and a mercury-mercury oxide electrode was used as a reference electrode. Cyclic voltammetry electrodeposition was carried out in an iridium plating solution with a scanning voltage of -0.6V to 0.6V, a scanning rate of 1 to 5mV / s, and a deposition temperature of 30 to 35°C.
8. The method for preparing an iridium composite-coated titanium anode according to claim 7, characterized in that: The iridium electroplating solution comprises iridium salt, potassium oxalate and a pH regulator, and the pH value of the iridium electroplating solution is 10-10.
5.
9. The method for preparing an iridium composite-coated titanium anode according to claim 1, characterized in that: Step S3 also includes high-temperature sintering. After the periodic electroplating is completed, the electroplated titanium plate is calcined at 250-350° C. for 1.5-2.5 hours to obtain an iridium composite-coated titanium anode.
10. An iridium composite-coated titanium anode prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Novel inert titanium anode and preparation method thereof
CN119859823A
A novel inert titanium anode and its preparation method
CN119859823B