Preparation method and application of Ce-MOF film layer on surface of magnesium alloy micro-arc oxidation film
By forming a Ce-MOF film layer on the surface of the magnesium alloy microarc oxide film on the surface of the magnesium alloy, the problems of poor corrosion resistance and difficulty in MOFs film formation are solved, and efficient corrosion resistance and safe and environmentally friendly preparation technology are achieved. It is suitable for Aerospace, automobile and other fields.
Patent Information
- Application Number
- CN202410984434.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Due to its high chemical and electrochemical activity and low standard electrode potential, magnesium alloys are prone to corrosion. Existing surface treatment technologies such as anodic oxide film and microarc oxide films have problems with loose porous properties and insufficient film corrosion resistance, and metal organic frames The material is difficult to form a film when applied to the surface of magnesium alloys, which limits its corrosion resistance.
The preparation method of Ce-MOF film layer on the surface of the magnesium alloy microarc oxide film is adopted. After microarc oxidation treatment, hydrothermal reaction is carried out in the in-situ growth liquid to form a uniform and dense Ce-MOF film layer, which is enhanced by Ce3+ and MOFs structures. The bonding force and corrosion resistance of the film layer.
It improves the corrosion resistance of magnesium alloys, shortens the preparation time, improves production efficiency, realizes safe, environmentally friendly and energy-saving processes, and expands the application range of magnesium alloys in aerospace, automobiles and other fields.
Smart Images

Figure CN118932456A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal surface protection treatment, and specifically relates to a preparation method and application of a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film. Background Art
[0002] Magnesium and magnesium alloys are green engineering materials in the 21st century. They have low density (1.8g / cm 3 ), high strength, large elastic modulus, good heat dissipation, good shock absorption, greater impact load bearing capacity than aluminum alloy, good resistance to organic and alkaline corrosion, good electrical and thermal conductivity, and good damping properties, etc. It is an indispensable and important basic material in the fields of aerospace, automobiles, computers, etc. However, magnesium alloys have high chemical and electrochemical activity and extremely low standard electrode potential, so their corrosion problem is the primary and core problem hindering the development of magnesium alloys.
[0003] At present, there are two main methods to improve the corrosion resistance of magnesium alloys. The first is to improve the corrosion resistance of the body of magnesium alloys, such as increasing the purity of the alloy and reducing harmful impurities in the alloy; the second is to use surface treatment technology to artificially form an isolation film on the surface of the base metal to directly block the contact between the base metal and the external environment, such as the more mature anodic oxide film and micro-arc oxide film (MAO). However, due to its loose and porous characteristics, the body of the magnesium alloy is easily pitted, resulting in poor corrosion resistance. For example, on magnesium alloys, there are some immature physical vapor deposition (PVD) and other technologies. Due to the large difference in the relative electrode potential between the coating and the magnesium substrate, the columnar crystals of the coating are difficult to eliminate, etc., the film does not improve the corrosion resistance of the magnesium alloy much, and sometimes even reduces it.
[0004] Metal-organic frameworks (MOFs) refer to porous structures formed by the interaction of metal clusters with organic ligands such as O and N; they are known for their extremely high specific surface area, excellent thermal stability and chemical stability. In recent years, some MOFs have been highly praised for their excellent water stability and have attracted interest in the field of corrosion protection. MOFs have satisfactory anti-corrosion performance, mainly due to the integration of MOFs particles as additives in polymer matrices. The application of MOFs particles can broaden its application prospects in the field of surface protection coatings, but this method is easily limited by the compatibility of MOFs crystals, resulting in poor dispersion stability of MOFs during coating preparation. Therefore, long-term exposure to corrosive media will form a weak interface, allowing corrosive ions to diffuse. In addition, the direct hydrothermal method in the prior art can only prepare MOFs powder, but cannot directly form a film on the surface of magnesium alloys, which greatly limits its application, that is, the application of MOFs anti-corrosion materials still faces the problem of poor binding force and inability to form a film. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems in the related art to a certain extent. To this end, the main purpose of the present invention is to provide a method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film, aiming to solve the problems that the existing MOFs are not widely used in magnesium alloy corrosion protection, there are many types of preparation raw materials, and the safety, environmental protection and energy-saving performance are poor. The present invention also provides the application of the Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film in the fields of aerospace, automobiles, medical equipment, 3C digital, etc.
[0006] The objective of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film comprises the following steps:
[0008] 1) immersing the magnesium alloy in a micro-arc oxidation growth solution for micro-arc oxidation treatment to obtain a magnesium alloy covered with a MAO layer;
[0009] 2) The magnesium alloy covered with the MAO layer is immersed in an in-situ growth solution for an in-situ hydrothermal reaction, and then cleaned and dried to obtain a magnesium alloy covered with a Ce-MOF film layer, namely, a Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film.
[0010] In some specific embodiments, the micro-arc oxidation growth solution is an aqueous solution including 0.03-0.06 M trisodium phosphate dodecahydrate and 0.1-0.3 M sodium hydroxide.
[0011] In some specific embodiments, the process parameters of the micro-arc oxidation treatment are: the temperature of the micro-arc growth liquid is 5-10° C., the reaction voltage is 300-400 V, and the reaction time is 2-8 min.
[0012] In some specific embodiments, the in-situ growth solution is an aqueous solution including 0.2-0.4 mM cerium nitrate hexahydrate and 0.3-0.5 mM terephthalic acid.
[0013] In some specific embodiments, the process parameters of the in-situ hydrothermal reaction are: reaction temperature is 110-130° C., and reaction time is 8-16 h.
[0014] In some specific embodiments, the process parameters of the in-situ hydrothermal reaction are: reaction temperature is 120-130° C., and reaction time is 10-14 h.
[0015] In some specific embodiments, the method further includes performing a grinding treatment on the magnesium alloy before performing the micro-arc oxidation treatment, specifically, firstly performing a grinding treatment on the magnesium alloy substrate, and then degreasing and deoiling the ground magnesium alloy substrate.
[0016] Furthermore, the degreasing and oil removal solution used in the degreasing and oil removal process is an aqueous solution including 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate in terms of mass volume concentration.
[0017] Furthermore, the polishing treatment specifically includes: polishing the magnesium alloy substrate using 150#, 600#, 800#, 1200#, and 2000# sandpaper respectively, and ultrasonically cleaning with alcohol and then drying.
[0018] A Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film prepared by the aforementioned preparation method is used in the fields of aerospace, automobiles, medical equipment and 3C digital technology.
[0019] Compared with the prior art, the present invention has at least the following advantages:
[0020] 1) The method for preparing the Ce-MOF film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided in the present application adopts a micro-arc oxidation growth liquid with specific components, whose components are simple and easy to obtain, which greatly shortens the time of micro-arc oxidation treatment to only 2-8 minutes, thereby greatly improving the production efficiency; at the same time, when preparing the Ce-MOF film layer, an aqueous solution is used as the medium, the temperature is low and the reaction time is short, making the production safer, more environmentally friendly and energy-saving;
[0021] 2) The method for preparing the Ce-MOF film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided by the present invention is to first perform micro-arc oxidation treatment on the magnesium alloy, and then use the traditional one-step hydrothermal method in a reactor to perform in-situ growth reaction on the magnesium alloy after micro-arc oxidation treatment to obtain a uniform and dense Ce-MOF film layer; the reagents used in the entire preparation process are simple, easy to obtain, and pollution-free to the environment. The overall process is simple and green and environmentally friendly, which can meet the needs of industrial development and mass production, and can further expand the application range of magnesium alloys. And the traditional one-step hydrothermal method is used, the reaction conditions are mild, and the process is stable; this makes the preparation method of the present invention more mature, more energy-saving, more practical for industrial production, simple to operate, etc., providing a new technical route for industrial production;
[0022] 3) The Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film prepared by the present invention is in-situ grown, and the prepared film layer is firmly bonded. The Ce-MOF grown on the micro-arc oxidation film layer as the substrate has good bonding force and film-forming properties, and the pores of the MAO film are closed, which not only introduces the rare earth Ce with corrosion inhibition effect, but also 3+ The structure of MOFs also increases the difficulty of corrosive ions entering the matrix, effectively blocking and preventing external corrosive ions (such as Cl -It can also protect the magnesium substrate by reducing the corrosion of the magnesium substrate, and is suitable for application in aerospace, automobile, medical equipment, 3C digital and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the specific embodiments of the present invention, the drawings required for use in the specific embodiments or the description of the prior art will be briefly introduced below.
[0024] Figure 1 is a scanning electron microscope photograph of the Ce-MOF film layer on the surface of the magnesium alloy in Example 1;
[0025] Figure 2 is a metallographic micrograph of the Ce-MOF film bonding strength test on the magnesium alloy surface in Example 1;
[0026] Figure 3 is the XRD spectrum of the Ce-MOF film layer on the surface of the magnesium alloy in Example 1;
[0027] Figure 4 AZ31 magnesium alloy, AZ31 magnesium alloy coated with MAO film and AZ31 magnesium alloy coated with Ce-MOF film are Tafel polarization curves at the same coordinates measured by an electrochemical workstation in Example 1;
[0028] Figure 5 is a scanning electron microscope photograph of the Ce-MOF film layer on the surface of the magnesium alloy in Example 2;
[0029] Figure 6 AZ31 magnesium alloy, AZ31 magnesium alloy coated with MAO film and AZ31 magnesium alloy coated with Ce-MOF film are Tafel polarization curves at the same coordinates measured by an electrochemical workstation in Example 2;
[0030] Figure 7 is a scanning electron microscope photograph of the Ce-MOF film layer on the surface of the magnesium alloy in Example 3;
[0031] Figure 8 These are the Tafel polarization curves of the AZ31 magnesium alloy, the AZ31 magnesium alloy coated with MAO film, and the AZ31 magnesium alloy coated with Ce-MOF film at the same coordinates measured by the electrochemical workstation in Example 3. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. The following embodiments are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.
[0033] When a certain amount, concentration or other value or parameter is expressed in the form of a range, a preferred range, or a preferred upper and lower numerical limit, it should be understood that it is equivalent to specifically revealing any range by combining any pair of upper range limits or preferred numerical values with any lower range limit or preferred numerical value, regardless of whether the range is specifically disclosed. Unless otherwise indicated, the numerical range values listed herein include the endpoints of the range, and all integers and fractions within the range.
[0034] Unless otherwise indicated, all percentages, parts, ratios, etc. herein are by weight.
[0035] The materials, methods, and examples herein are illustrative and are not to be construed as limiting unless specifically stated.
[0036] The test methods used in the following embodiments include:
[0037] The corrosion resistance and bonding strength are reflected by testing the Tafel polarization curve of each test sample and metallographic microscopic observation of the scratch.
[0038] 1) Binding strength test;
[0039] A metallographic microscope (Zeiss, Germany) was used to form a criss-cross pattern on the surface of different coatings using a QFH-type cutter. The cut reached the Mg substrate, and then its surface was carefully cleaned five times with a brush, and tape was stuck on the cut to pull it apart. The adhesion between the coating and the AZ31 substrate was evaluated according to GB / T 9286-1998.
[0040] Example 1
[0041] The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film provided in this embodiment comprises the following steps:
[0042] 1) Degreasing and oil removal
[0043] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;
[0044] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;
[0045] 13) Soak the polished magnesium alloy AZ31 in the above degreasing and deoiling aqueous solution, keep it in a water bath at 50°C for 60 seconds, then wash it with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polish it with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 2 minutes; then wash it once with deionized water and blow it dry with cold air;
[0046] 2) Micro-arc oxidation film (MAO for short)
[0047] 21) Prepare a micro-arc oxidation growth solution containing 0.049 M trisodium phosphate dodecahydrate and 0.18 M sodium hydroxide using deionized water according to the molar concentration;
[0048] 22) First, the magnesium alloy sample after degreasing and deoiling in step 1) is fixed in a polymethyl methacrylate electrolytic cell equipped with a stainless steel plate by copper wire, and then the micro-arc oxidation growth solution in step 21) is poured; the anode is AZ31 magnesium alloy, and the cathode is a stainless steel plate; the growth solution temperature is 8°C, the reaction voltage is 350V, and the reaction time is 5min, to obtain a magnesium alloy covered with a MAO film;
[0049] 3) In situ growth of Ce-MOF film (abbreviated as Ce-MOF)
[0050] 31) Using deionized water, prepare an in-situ growth solution containing 0.2 mM cerium nitrate hexahydrate and 0.4 mM terephthalic acid according to the molar concentration;
[0051] 32) placing the magnesium alloy with the surface MAO layer prepared in step 2) into a polytetrafluoroethylene liner sleeve, then pouring the in-situ growth solution prepared in step 31) into the liner and placing the liner into the reactor, tightening it, and finally placing it in a drying oven for in-situ growth, the reaction temperature is 120° C., the reaction time is 12 h, and then washing and drying to obtain a magnesium alloy covered with a Ce-MOF film, i.e., a Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film;
[0052] The cleaning and drying specifically comprises the following steps: firstly cleaning the magnesium alloy sample covered with the Ce-MOF film layer after the reaction in step 3) with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then placing it in an ultrasonic cleaning machine for ultrasonic cleaning in anhydrous ethanol for 7 minutes, and then cleaning it with deionized water and drying it to obtain the Ce-MOF film layer (Ce-MOF film layer) on the surface of the magnesium alloy micro-arc oxidation film.
[0053] The present application conducts structural and morphological tests on the Ce-MOF film layer on the magnesium alloy surface prepared in this embodiment, specifically:
[0054] 1) Appearance
[0055] The present application conducted an appearance morphology test on the Ce-MOF film layer on the magnesium alloy surface in Example 1, and the electron microscope scanning image thereof is shown in FIG. Figure 1 As shown in the figure, the surface of the Ce-MOF film on the magnesium alloy is completely covered but not very smooth, which may be related to the Ce 3+ It is related to the coordination binding between ions and organic ligands (terephthalic acid).
[0056] In addition, the metallographic micrograph of the Ce-MOF film layer on the magnesium alloy surface is shown in Figure 2 As shown in the figure, it can be seen that the Ce-MOF film layer has a clear and smooth cutting edge, no obvious large-scale detachment is observed, and the small detachment area in the intersection area does not exceed 5%. According to the classification standard of bonding strength, the bonding strength between the Ce-MOF film layer and the magnesium alloy is evaluated as level 1.
[0057] 2) Structural analysis
[0058] The present application tests the crystallinity of the Ce-MOF film layer on the magnesium alloy surface in Example 1, and its XRD spectrum is as follows: Figure 3 As shown in the figure, the Ce-MOF film layer on the magnesium alloy surface has multiple characteristic diffraction peaks at 6.7°, 28°, 28.5°, 33°, 47.5° and 56.5°, which are consistent with the CeO 2 These peaks are mostly sharp, indicating that Ce-MOF has good crystallinity.
[0059] 3) Electrochemical performance
[0060] The present application tests the electrochemical properties of the magnesium alloy surface film layer in Example 1 by using an electrochemical workstation, specifically:
[0061] The Tafel polarization curves of magnesium alloy AZ31, magnesium alloy coated with MAO film (curve MAO) and magnesium alloy coated with Ce-MOF film (curve Ce-MOF) measured by electrochemical workstation at the same coordinates are as follows: Figure 4 Specifically:
[0062] The corrosion resistance test of the magnesium alloy protective film is represented by the electrochemical polarization curve (equipment model is Princeton4000A), in which the corrosion voltage of AZ31 magnesium alloy is -1.37V, the corrosion voltage of AZ31 magnesium alloy covered with MAO film after treatment under the conditions of Example 1 is -1.55V, and the corrosion voltage of AZ31 magnesium alloy covered with Ce-MOF film is -1.05V. Compared with the magnesium alloy substrate, the corrosion voltage is significantly improved, the corrosion tendency is reduced, and the corrosion rate and corrosion resistance are directly related to the corrosion current density. The corrosion current density of pure AZ31 magnesium alloy is 1.02×10 -5 Acm -2 The corrosion current density of the magnesium alloy covered with MAO film is 7.31×10 -7 A cm -2 However, the corrosion current density of the sample covered with Ce-MOF film after treatment under the conditions of Example 1 is 3.75×10 -8 A cm -2The corrosion current density of the treated sample is reduced by three orders of magnitude compared with that of the AZ31 magnesium alloy sample. The above results fully demonstrate that the Ce-MOF film has an effective corrosion inhibition effect on the AZ31 magnesium alloy. The Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film of the present invention has excellent corrosion resistance and can effectively protect the magnesium substrate.
[0063] Example 2
[0064] The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film provided in this embodiment comprises the following steps:
[0065] 1) Degreasing and oil removal
[0066] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;
[0067] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;
[0068] 13) The polished magnesium alloy AZ31 was immersed in the above-mentioned degreasing and deoiling aqueous solution, kept in a water bath at 50°C for 60 seconds, then alkaline washed with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polished with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 2 minutes; then rinsed once with deionized water and blown dry with cold air.
[0069] 2) Micro-arc oxidation film (MAO for short)
[0070] 21) Prepare a micro-arc oxidation growth solution containing 0.049 M trisodium phosphate dodecahydrate and 0.18 M sodium hydroxide using deionized water according to the molar concentration;
[0071] 22) First, the magnesium alloy sample after degreasing and deoiling in step 1) is fixed in a polymethyl methacrylate electrolytic cell equipped with a stainless steel plate by copper wire, and then the micro-arc oxidation growth solution in step 21) is poured; the anode is AZ31 magnesium alloy, and the cathode is a stainless steel plate; the growth solution temperature is 8°C, the reaction voltage is 350V, and the reaction time is 5min, to obtain a magnesium alloy covered with a MAO film;
[0072] 3) In situ growth of Ce-MOF film (abbreviated as Ce-MOF)
[0073] 31) using deionized water to prepare an in-situ growth solution containing 0.3 mM cerium nitrate hexahydrate and 0.3 mM terephthalic acid according to the molar concentration;
[0074] 32) placing the magnesium alloy with the surface MAO layer prepared in step 2) into a polytetrafluoroethylene liner sleeve, then pouring the in-situ growth solution prepared in step 31) into the liner and placing the liner into the reactor, tightening it, and finally placing it in a drying oven for in-situ growth, the reaction temperature is 110° C., the reaction time is 10 h, and a magnesium alloy covered with a Ce-MOF film is obtained, i.e., a Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film;
[0075] The cleaning and drying are as follows: the magnesium alloy sample covered with the Ce-MOF film layer after the reaction in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then ultrasonically cleaned in anhydrous ethanol for 6 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain the Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film.
[0076] The present application conducts structural and morphological tests on the Ce-MOF film layer on the magnesium alloy surface prepared in this embodiment, specifically:
[0077] 1) Appearance
[0078] The present application conducted an appearance morphology test on the Ce-MOF film layer on the magnesium alloy surface in Example 2, and the electron microscope scanning image thereof is shown in FIG. Figure 5 As shown in the figure, it can be seen that the surface of the Ce-MOF film layer on the magnesium alloy is completely covered, the flaky Ce-MOF is relatively thin, and most of them grow perpendicular to the alloy surface.
[0079] 2) Electrochemical performance
[0080] The present application tests the electrochemical properties of the magnesium alloy surface film layer in Example 2 by using an electrochemical workstation, specifically:
[0081] The Tafel polarization curves of magnesium alloy AZ31, magnesium alloy coated with MAO film (curve MAO) and magnesium alloy coated with Ce-MOF film (curve Ce-MOF) measured by electrochemical workstation at the same coordinates are as follows: Figure 6 As shown, specifically:
[0082] The corrosion resistance test of the magnesium alloy protective film is represented by the electrochemical polarization curve (equipment model is Princeton4000A), in which the corrosion voltage of AZ31 magnesium alloy is -1.37V, the corrosion voltage of AZ31 magnesium alloy covered with MAO film after treatment under the conditions of Example 2 is -1.55V, and the corrosion voltage of AZ31 magnesium alloy covered with Ce-MOF film is -0.95V. Compared with the magnesium alloy substrate, the corrosion voltage is significantly improved, the corrosion tendency is reduced, and the corrosion rate and corrosion resistance are directly related to the corrosion current density. The corrosion current density of pure AZ31 magnesium alloy is 1.02×10 -5 Acm -2The corrosion current density of the magnesium alloy covered with MAO film is 7.31×10 -7 A cm -2 However, the corrosion current density of the sample covered with Ce-MOF film after treatment under the conditions of Example 2 is 7.65×10 -8 A cm -2 The corrosion current density of the treated sample is reduced by three orders of magnitude compared with that of the AZ31 magnesium alloy sample. The above results fully demonstrate that the Ce-MOF film has an effective corrosion inhibition effect on the AZ31 magnesium alloy. The Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film of the present invention has excellent corrosion resistance and can effectively protect the magnesium substrate.
[0083] Example 3
[0084] The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film provided in this embodiment comprises the following steps:
[0085] 1) Degreasing and oil removal
[0086] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;
[0087] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;
[0088] 13) The polished magnesium alloy AZ31 was immersed in the above-mentioned degreasing and deoiling aqueous solution, kept in a water bath at 50°C for 60 seconds, then alkaline washed with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polished with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 2 minutes; then rinsed once with deionized water and blown dry with cold air.
[0089] 2) Micro-arc oxidation film (MAO for short)
[0090] 21) Prepare a micro-arc oxidation growth solution containing 0.049 M trisodium phosphate dodecahydrate and 0.18 M sodium hydroxide using deionized water according to the molar concentration;
[0091] 22) First, the magnesium alloy sample after degreasing and deoiling in step 1) is fixed in a polymethyl methacrylate electrolytic cell equipped with a stainless steel plate by copper wire, and then the micro-arc oxidation growth solution in step 21) is poured in; the anode is AZ31 magnesium alloy, and the cathode is a stainless steel plate; the growth solution temperature is 8°C, the reaction voltage is 350V, and the reaction time is 5min, to obtain a MAO layer on the surface of the magnesium alloy;
[0092] 3) In situ growth of Ce-MOF film (abbreviated as Ce-MOF)
[0093] 31) using deionized water to prepare an in-situ growth solution containing 0.4 mM cerium nitrate hexahydrate and 0.5 mM terephthalic acid according to the molar concentration;
[0094] 32) placing the magnesium alloy with the surface MAO layer prepared in step 2) into a polytetrafluoroethylene liner sleeve, then pouring the in-situ growth liquid prepared in step 31) into the liner and placing the liner into a reactor, tightening it, and finally placing it in a drying oven for in-situ growth, with a reaction temperature of 130° C. and a reaction time of 8 h, to obtain a Ce-MOF film layer on the surface of the magnesium alloy, i.e., a Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film;
[0095] The cleaning and drying are as follows: the magnesium alloy sample covered with the Ce-MOF film layer after the reaction in step 3) is first cleaned with flowing deionized water to remove the in-situ growth liquid attached to the surface, and then the sample is ultrasonically cleaned in anhydrous ethanol for 8 minutes using an ultrasonic cleaning machine, and then cleaned with deionized water and dried to obtain the Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film.
[0096] The present application conducts structural and morphological tests on the Ce-MOF film layer on the magnesium alloy surface prepared in this embodiment, specifically:
[0097] 1) Appearance
[0098] The present application conducted an appearance morphology test on the Ce-MOF film layer on the magnesium alloy surface in Example 1, and the electron microscope scanning image thereof is shown in FIG. Figure 7 As shown in the figure, it can be seen that the surface of the Ce-MOF film layer on the magnesium alloy is completely covered, the flaky Ce-MOF becomes thicker, and the growth direction is different.
[0099] 2) Electrochemical performance
[0100] The present application tests the electrochemical properties of the magnesium alloy surface film layer in Example 3 by using an electrochemical workstation, specifically:
[0101] The Tafel polarization curves of magnesium alloy AZ31, magnesium alloy coated with MAO film (curve MAO) and magnesium alloy coated with Ce-MOF film (curve Ce-MOF) measured by electrochemical workstation at the same coordinates are as follows: Figure 8 As shown, specifically:
[0102] The corrosion resistance test of the magnesium alloy protective film is represented by the electrochemical polarization curve (equipment model is Princeton4000A), in which the corrosion voltage of AZ31 magnesium alloy is -1.37V, the corrosion voltage of AZ31 magnesium alloy covered with MAO film after treatment under the conditions of Example 1 is -1.55V, and the corrosion voltage of AZ31 magnesium alloy covered with Ce-MOF film is -0.90V. Compared with the magnesium alloy substrate, the corrosion voltage is significantly improved, the corrosion tendency is reduced, and the corrosion rate and corrosion resistance are directly related to the corrosion current density. The corrosion current density of pure AZ31 magnesium alloy is 1.02×10 -5 Acm -2 The corrosion current density of the magnesium alloy covered with MAO film is 7.31×10 -7 A cm -2 However, the corrosion current density of the sample covered with Ce-MOF film after treatment under the conditions of Example 3 is 8.65×10 -8 A cm -2 The corrosion current density of the treated sample is reduced by three orders of magnitude compared with that of the AZ31 magnesium alloy sample. The above results fully demonstrate that the Ce-MOF film has an effective corrosion inhibition effect on the AZ31 magnesium alloy. The Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film of the present invention has excellent corrosion resistance and can effectively protect the magnesium substrate.
[0103] Comparative Example 1
[0104] The method for preparing the Ce-MOF film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided in this comparative example is basically the same as that of Example 2, except that the magnesium alloy is not subjected to micro-arc oxidation treatment, and the Ce-MOF film is directly grown in situ on the magnesium alloy, and specifically comprises the following steps:
[0105] 1) Degreasing and oil removal
[0106] 11) preparing an aqueous solution containing 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate;
[0107] 12) Pretreatment of magnesium alloy: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy, and using alcohol to ultrasonically clean it for five minutes and then dry it for use;
[0108] 13) The polished magnesium alloy AZ31 was immersed in the above-mentioned degreasing and deoiling aqueous solution, kept in a water bath at 50°C for 60 seconds, then alkaline washed with a 1M sodium hydroxide aqueous solution for 30 seconds, and then polished with 400g / L nitric acid (ρ=1.42g / ml) at room temperature 25°C for 1-2min; then rinsed once with deionized water and blown dry with cold air.
[0109] 2) In situ growth of Ce-MOF film (abbreviated as Ce-MOF)
[0110] 21) using deionized water to prepare an in-situ growth solution containing 0.3 mM cerium nitrate hexahydrate and 0.3 mM terephthalic acid according to the molar concentration;
[0111] 22) The magnesium alloy pretreated in step 1) is placed in a polytetrafluoroethylene inner liner sleeve, and then the in-situ growth liquid prepared in step 21) is poured in and the inner liner is placed in a reactor, tightened, and finally placed in a drying oven for in-situ growth. The reaction temperature is 110°C and the reaction time is 10 hours. As a result, Ce-MOF nanoparticles are dispersed and arranged on the surface of the magnesium alloy, and it is impossible to obtain a magnesium alloy covered with a Ce-MOF film, and only MOFs powder can be obtained in some areas.
[0112] By comparing Example 2 with Comparative Example 1, it can be seen that in the method for preparing the Ce-MOF film layer on the surface of the micro-arc oxidation film of the magnesium alloy provided in the present application, the magnesium alloy is first subjected to MAO film treatment, which is a prerequisite for realizing the hydrothermal method to prepare the Ce-MOF film layer, that is, the micro-arc oxidation treatment and the in-situ hydrothermal reaction are synergistic, and the preparation of the Ce-MOF film layer is successfully realized, and the Ce-MOF film layer has excellent bonding with the magnesium alloy AZ31.
[0113] In summary, the preparation method of the Ce-MOF film layer on the surface of the magnesium alloy micro-arc film provided by the present invention is based on the magnesium alloy MAO film, and a Ce-MOF film layer is in situ grown by a hydrothermal method, which not only introduces the rare earth Ce with corrosion inhibition effect, but also 3+ , and the structure of MOFs increases the difficulty of corrosive ions entering the matrix; in addition, due to in-situ growth, the bonding strength between the film layer and the matrix and the film-forming performance are also improved accordingly, which improves the feasibility of industrial application. The Ce-MOF film layer not only closes the pores of the MAO film layer, but also has the characteristics of easy modification and corrosion resistance. Its performance is far better than that of the untreated magnesium alloy AZ31. After a large number of experiments, the inventors found that using a traditional mature reactor on the MAO film layer can achieve the purpose through hydrothermal reaction, and generate a Ce-MOF film layer with good bonding strength and good corrosion resistance.
[0114] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention.
Claims
1. A method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film, characterized in that: The steps include: 1) immersing the magnesium alloy in a micro-arc oxidation growth solution for micro-arc oxidation treatment to obtain a magnesium alloy covered with a MAO layer; 2) The magnesium alloy covered with the MAO layer is immersed in an in-situ growth solution for an in-situ hydrothermal reaction, and then cleaned and dried to obtain a magnesium alloy covered with a Ce-MOF film layer, namely, a Ce-MOF film layer on the surface of the magnesium alloy micro-arc oxidation film.
2. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 1, characterized in that: The micro-arc oxidation growth liquid is an aqueous solution including 0.03-0.06M trisodium phosphate dodecahydrate and 0.1-0.3M sodium hydroxide.
3. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 1, characterized in that: The process parameters of the micro-arc oxidation treatment are: the temperature of the micro-arc growth liquid is 5-10° C., the reaction voltage is 300-400 V, and the reaction time is 2-8 min.
4. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 1, characterized in that: The in-situ growth solution is an aqueous solution including 0.2-0.4 mM cerium nitrate hexahydrate and 0.3-0.5 mM terephthalic acid.
5. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 4, characterized in that: The process parameters of the in-situ hydrothermal reaction are: reaction temperature of 110-130° C., and reaction time of 8-16 h.
6. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 1, characterized in that: The method also includes pre-treatment of the magnesium alloy before micro-arc oxidation treatment, specifically, grinding the magnesium alloy substrate first, and then degreasing and deoiling the ground magnesium alloy substrate.
7. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 6, characterized in that: The grinding treatment specifically includes: using 150#, 600#, 800#, 1200#, and 2000# sandpaper to grind the magnesium alloy substrate, and using alcohol to perform ultrasonic cleaning and then drying.
8. The method for preparing a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film according to claim 6, characterized in that: The degreasing and oil removal solution used in the degreasing and oil removal process is an aqueous solution including 40 g / L of sodium hydroxide, 25 g / L of sodium carbonate, and 40 g / L of sodium phosphate, based on mass volume concentration.
9. Application of a Ce-MOF film layer on the surface of a magnesium alloy micro-arc oxidation film prepared by the preparation method according to any one of claims 1 to 8 in the fields of aerospace, automobile, medical equipment and 3C digital.